Preparation and Characterization of Sodium-Ion Battery Separators Using Carboxymethyl Cellulose Sodium and Polyacrylic Acid Aerogels

In recent years, the global demand for advanced energy storage solutions has surged, driven by the proliferation of portable electronics, the expansion of electric vehicles, and the growing need for grid-scale energy storage. Lithium-ion batteries have dominated this landscape due to their high energy density and long cycle life. However, concerns over the limited availability and uneven geographical distribution of lithium resources have spurred intense research into alternative battery chemistries. Sodium-ion batteries have emerged as a promising candidate, owing to the abundance, low cost, and similar electrochemical behavior of sodium compared to lithium. The core components of a sodium-ion battery, including electrodes, electrolytes, and separators, must be optimized to achieve performance parity or superiority over lithium-based systems. Among these, the separator plays a critical role in preventing electrical short circuits while facilitating ionic transport. Traditional polyolefin separators, though widely used, suffer from poor thermal stability, inadequate wettability with organic electrolytes, and safety risks. Glass fiber separators, often employed in research settings, exhibit high porosity but poor mechanical integrity and significant electrolyte leakage. Therefore, developing novel separator materials with enhanced properties is crucial for advancing sodium-ion battery technology.

Cellulose-based materials offer a sustainable and high-performance alternative for battery separators. Derived from abundant natural resources, cellulose and its derivatives boast excellent chemical stability, thermal resistance, and tunable porosity. Carboxymethyl cellulose sodium (CMC), a water-soluble cellulose derivative, contains carboxylate groups that can enhance sodium ion conduction. Polyacrylic acid (PAA), another water-soluble polymer, provides functional carboxyl groups that can undergo cross-linking reactions. By combining CMC and PAA, we can fabricate aerogel structures with tailored pore architectures through simple sol-gel and freeze-drying processes. Aerogels, known for their ultra-low density and high surface area, can serve as ideal separator matrices due to their interconnected porous networks, which promote electrolyte uptake and uniform ion flux. In this study, we aim to design and characterize a novel aerogel-based separator for sodium-ion batteries using CMC and PAA. We investigate the effects of cross-linking temperature on the structural, mechanical, and electrochemical properties of the separator, with the goal of surpassing the performance of conventional glass fiber separators. Our approach emphasizes environmental friendliness, cost-effectiveness, and scalability, aligning with the broader objectives of sustainable energy storage development.

The successful implementation of high-performance separators could significantly impact the commercialization of sodium-ion batteries. By improving ionic conductivity, thermal stability, and safety, such separators can enable longer battery lifespans, faster charging rates, and operation under extreme conditions. This research contributes to the ongoing efforts to overcome the limitations of current sodium-ion battery components, paving the way for their adoption in large-scale applications. Through detailed material characterization and electrochemical testing, we demonstrate the potential of CMC-PAA aerogels as next-generation separators, offering insights into structure-property relationships that guide future optimization.

Materials and Experimental Methods

To fabricate the aerogel separators, we selected carboxymethyl cellulose sodium (CMC) with a viscosity of 600–1000 mPa·s and a 50 wt% aqueous solution of polyacrylic acid (PAA) with an average molecular weight of 3000. These materials were chosen for their water solubility, functional groups, and compatibility with green processing. Additional chemicals included sodium metal (anode material), sodium alginate (binder), anhyd ethanol, n-butanol, and a sodium-ion electrolyte composed of 1 M sodium perchlorate in a mixture of ethylene carbonate and propylene carbonate (EC/PC, 1:1 by volume). Hard carbon served as the active material for the negative electrode, while copper foil and conductive carbon black were used for current collection. Commercial GF/D glass fiber separators were used as benchmarks. All materials were handled in controlled environments to prevent contamination.

The separator preparation began by dissolving 2.00 g of CMC in 96 mL of deionized water under continuous stirring for 20 minutes. Then, 2.00 mL of the PAA solution was added dropwise, and stirring continued for another 20 minutes to ensure homogeneous mixing. The resulting solution was subjected to ultrasonic degassing for 30 minutes to remove air bubbles, which could defect the gel structure. The solution was then allowed to gel at room temperature for 5 days, forming a robust hydrogel. The hydrogel was shaped into thin sheets and pre-frozen at −20 °C to stabilize the structure. Freeze-drying was conducted at −20 °C for 24 hours, yielding porous aerogel sheets with a thickness of approximately 1.2 mm. These sheets were cut into circular discs of 18 mm diameter using a hollow punch. To enhance mechanical strength and stabilize the pore structure, the aerogels were thermally cross-linked at different temperatures: 105, 130, 140, and 150 °C for 4 hours each. The resulting separators were denoted as 105°C-CMC-PAA, 130°C-CMC-PAA, 140°C-CMC-PAA, and 150°C-CMC-PAA, respectively.

For electrochemical evaluation, we assembled sodium-ion half-cells in an argon-filled glove box. The negative electrode was prepared by mixing hard carbon, conductive carbon black, and sodium alginate binder in a mass ratio of 90:5:5. The mixture was dispersed in deionized water, ground thoroughly, and coated onto copper foil. After drying at 65 °C for 12 hours, the electrode was cut into 12 mm diameter discs. The cell assembly used sodium metal as the counter/reference electrode, the prepared CMC-PAA aerogel or glass fiber as the separator, and the NaClO4/EC/PC electrolyte. CR2032 coin cells were crimped and aged for 24 hours before testing to ensure proper electrolyte wetting.

We employed a comprehensive suite of characterization techniques to assess the separators. The wettability was evaluated by measuring the contact angle of the EC/PC solvent on the separator surface using an optical tensiometer. Thermal stability was analyzed via thermogravimetric analysis (TGA) under a nitrogen atmosphere, with heating from room temperature to 600 °C at a rate of 10 °C/min. The morphological features were examined using scanning electron microscopy (SEM) at various magnifications to observe surface and cross-sectional pore structures. Fourier-transform infrared spectroscopy (FTIR) was performed in the range of 4000–300 cm−1 to identify chemical bonds and cross-linking effects.

Mechanical properties were assessed through tensile testing on strip-shaped samples (12 mm × 45 mm) at a constant crosshead speed of 1 mm/min. The elongation at break was recorded as an indicator of flexibility and durability. Porosity was determined by the n-butanol absorption method, where the separator was immersed in n-butanol, and the mass change was measured. The porosity \( P \) is calculated as:

$$ P = \frac{m_1 – m_0}{\rho V} \times 100\% $$

Here, \( m_0 \) and \( m_1 \) are the masses before and after immersion, \( \rho \) is the density of n-butanol, and \( V \) is the geometric volume of the separator.

Electrolyte uptake \( A \) was evaluated by soaking the separator in the NaClO4/EC/PC electrolyte and weighing:

$$ A = \frac{m_1 – m_0}{m_0} \times 100\% $$

where \( m_0 \) and \( m_1 \) are the dry and wet masses, respectively.

The electrolyte leakage rate \( S’ \) was measured by placing a separator saturated with electrolyte under a 200 g weight and monitoring the mass loss over time:

$$ S’ = \frac{M_0 – M_1}{M_0} \times 100\% $$

with \( M_0 \) and \( M_1 \) being the electrolyte absorption masses before and after applying the weight.

Electrochemical impedance spectroscopy (EIS) was conducted using a two-electrode configuration with stainless steel blocking electrodes. The frequency range was 1 MHz to 0.1 Hz with a small AC amplitude. The bulk resistance \( R \) of the separator was derived from the high-frequency intercept on the real axis. The ionic conductivity \( \gamma \) was then computed as:

$$ \gamma = \frac{d}{R S} $$

where \( d \) is the separator thickness, and \( S \) is the contact area. All EIS measurements were performed on electrolyte-soaked separators at room temperature.

Galvanostatic charge-discharge testing of the half-cells was carried out at various current densities ranging from 25 to 1000 mA/g. The specific capacity, cycling stability, and rate capability were evaluated. Coulombic efficiency was monitored to assess reversibility. All tests were repeated with at least three samples to ensure statistical reliability.

Results and Analysis

Physical and Chemical Properties

The aerogel separators exhibited a white, lightweight, and flexible appearance. Upon contact with the EC/PC electrolyte, all separators showed instant wetting, with contact angles dropping to nearly zero within 0.033 seconds. This super-wettability is attributed to the hydrophilic nature of CMC and PAA, which contain polar hydroxyl and carboxyl groups. The electrolyte uptake exceeded 900% for all samples, indicating a highly porous structure capable of retaining ample electrolyte for ion transport. Such high uptake is beneficial for sodium-ion battery operation, as it reduces internal resistance and enhances electrode-electrolyte interaction.

Thermal analysis revealed that the separators are stable up to approximately 155 °C. The TGA curves displayed an initial weight loss below 100 °C due to moisture evaporation, followed by a plateau. Decomposition of polymer chains occurred above 155 °C, with maximum degradation rates around 330 °C. The cross-linked samples (130°C-CMC-PAA, 140°C-CMC-PAA, 150°C-CMC-PAA) showed slightly higher thermal stability than the non-cross-linked 105°C-CMC-PAA, as evidenced by a shift in derivative peaks. This improvement is due to the formation of ester bonds between CMC and PAA during thermal treatment, which enhances network rigidity. When subjected to elevated temperatures (up to 205 °C) for 2 hours, the separators maintained dimensional stability without significant shrinkage, underscoring their suitability for high-temperature sodium-ion battery applications.

FTIR spectroscopy confirmed chemical interactions between CMC and PAA. Characteristic peaks included broad O–H stretching around 3400 cm−1, C–H stretching at 2817 cm−1, asymmetric and symmetric carboxylate stretches at 1605 and 1422 cm−1, and ester C=O and C–O–C stretches at 1743 and 1270 cm−1. Comparing spectra from 105°C-CMC-PAA and 130°C-CMC-PAA, the intensity of O–H and carboxylate peaks decreased with higher cross-linking temperature, indicating consumption of these groups in esterification reactions. This corroborates the enhancement of cross-linking density with temperature.

Mechanical testing showed that the elongation at break varied with cross-linking temperature. The values are summarized in Table 1. Initially, increasing temperature improved flexibility due to better network formation, but excessive cross-linking led to brittleness. The optimal balance was achieved at 130–140 °C.

Table 1: Mechanical Properties of CMC-PAA Aerogel Separators
Separator Type Elongation at Break (%) Tensile Strength (MPa)
105°C-CMC-PAA 13.06 ± 0.5 1.2 ± 0.1
130°C-CMC-PAA 16.35 ± 0.6 1.8 ± 0.2
140°C-CMC-PAA 16.36 ± 0.7 1.9 ± 0.2
150°C-CMC-PAA 12.70 ± 0.4 2.1 ± 0.3

SEM imaging revealed a three-dimensional interconnected porous network with pore sizes ranging from 20 to 200 μm. The pores were honeycomb-like and uniformly distributed, resulting from ice-templating during freeze-drying. As cross-linking temperature increased, a slight reduction in average pore size and porosity was observed, consistent with network contraction. Porosity measurements, detailed in Table 2, aligned with these observations.

Table 2: Porosity and Pore Characteristics of Separators
Separator Type Porosity (%) Average Pore Size (μm)
105°C-CMC-PAA 78.93 ± 1.2 180 ± 20
130°C-CMC-PAA 76.99 ± 1.0 150 ± 15
140°C-CMC-PAA 75.45 ± 1.1 140 ± 15
150°C-CMC-PAA 74.12 ± 1.3 130 ± 10

Electrochemical Performance

The sodium-ion half-cells with CMC-PAA separators demonstrated excellent electrochemical behavior. Rate capability tests, conducted at current densities from 25 to 1000 mA/g, are summarized in Table 3. The 130°C-CMC-PAA separator delivered the highest specific capacities across all rates, outperforming the glass fiber separator. For instance, at 25 mA/g, the charging specific capacity was 345.8 mA·h/g, compared to 279.0 mA·h/g for glass fiber. Even at high rates like 1000 mA/g, the capacity retention was superior, indicating efficient ion transport kinetics.

Table 3: Charging Specific Capacities at Different Current Densities
Current Density (mA/g) 130°C-CMC-PAA (mA·h/g) Glass Fiber (mA·h/g) 105°C-CMC-PAA (mA·h/g) 140°C-CMC-PAA (mA·h/g) 150°C-CMC-PAA (mA·h/g)
25 345.8 ± 5.2 279.0 ± 4.1 320.5 ± 4.8 335.2 ± 5.0 338.6 ± 5.1
50 317.3 ± 4.8 233.1 ± 3.5 295.1 ± 4.4 305.8 ± 4.6 310.4 ± 4.7
100 274.2 ± 4.1 190.5 ± 2.9 250.3 ± 3.8 265.7 ± 4.0 268.9 ± 4.0
250 136.8 ± 2.1 105.9 ± 1.6 125.4 ± 1.9 130.2 ± 2.0 132.5 ± 2.0
500 84.8 ± 1.3 69.6 ± 1.0 78.2 ± 1.2 81.5 ± 1.2 82.7 ± 1.2
1000 61.8 ± 0.9 49.4 ± 0.7 56.9 ± 0.9 59.3 ± 0.9 60.1 ± 0.9
25 (return) 341.4 ± 5.1 275.1 ± 4.1 315.8 ± 4.7 330.5 ± 5.0 334.2 ± 5.0

Cycling stability tests at 50 mA/g over 55 cycles revealed that the 130°C-CMC-PAA separator maintained 92.5% of its initial capacity, with Coulombic efficiency consistently near 100%. In contrast, the glass fiber separator retained only 85% under identical conditions. The enhanced cycling performance is attributed to the stable porous structure and good interfacial contact provided by the aerogel separator, which minimizes polarization and side reactions.

EIS measurements yielded Nyquist plots with a single semicircle in the high-frequency region, corresponding to the bulk resistance of the separator soaked with electrolyte. The calculated ionic conductivities and resistances are presented in Table 4. The 130°C-CMC-PAA separator exhibited an ionic conductivity of 1.877 mS/cm, which is lower than that of glass fiber (6.596 mS/cm) but higher than many commercial polyolefin separators (typically 0.1–0.8 mS/cm). This conductivity is sufficient for efficient operation in sodium-ion batteries, especially when combined with the separator’s high electrolyte uptake and low leakage.

Table 4: Ionic Conductivity and Resistance of Separators
Separator Type Resistance (Ω) Ionic Conductivity (mS/cm) Electrolyte Leakage Rate (%)
105°C-CMC-PAA 12.48 ± 0.2 1.079 ± 0.02 0.58 ± 0.05
130°C-CMC-PAA 5.52 ± 0.1 1.877 ± 0.03 0.42 ± 0.04
140°C-CMC-PAA 10.40 ± 0.2 1.143 ± 0.02 0.51 ± 0.05
150°C-CMC-PAA 5.32 ± 0.1 1.928 ± 0.03 0.64 ± 0.06
Glass Fiber 2.70 ± 0.1 6.596 ± 0.10 1.032 ± 0.10

The electrolyte leakage rate, a critical safety parameter, was significantly lower for CMC-PAA separators (0.42–0.64%) than for glass fiber (1.032%). This reduction minimizes the risk of electrolyte drying, short circuits, and thermal runaway in sodium-ion batteries. The combination of moderate ionic conductivity and low leakage contributes to the overall superior electrochemical performance of the 130°C-CMC-PAA separator.

Discussion on Structure-Performance Relationships

The performance of a sodium-ion battery separator is governed by its microstructure, chemical composition, and interaction with the electrolyte. In this study, the CMC-PAA aerogel separators displayed a tunable porous architecture influenced by cross-linking temperature. As temperature increased, ester cross-linking between CMC hydroxyls and PAA carboxyls intensified, leading to a denser network with slightly smaller pores and lower porosity. This structural evolution impacts multiple properties. First, the reduced pore size can enhance mechanical strength and provide better resistance to dendrite penetration, a common issue in sodium-ion batteries. Second, the maintained high porosity (above 74%) ensures ample electrolyte storage, facilitating ion conduction. The optimal balance was achieved at 130 °C, where cross-linking improved thermal and mechanical stability without excessively compromising pore connectivity.

The ionic conductivity of a separator is described by the equation:

$$ \gamma = n \mu q $$

where \( n \) is the charge carrier concentration, \( \mu \) is the mobility, and \( q \) is the charge. In CMC-PAA separators, the carboxylate groups from CMC may dissociate to provide sodium ions, potentially increasing \( n \). Moreover, the hydrophilic pores promote electrolyte infiltration, enhancing \( \mu \). However, the conductivity values were lower than those of glass fiber, likely due to the larger pore size and lower tortuosity of glass fiber, which offers less resistance to ion flow. Nonetheless, the CMC-PAA separators’ conductivity surpasses that of many polymer-based separators, making them viable for practical sodium-ion battery applications.

Electrochemical performance, particularly rate capability, is closely tied to separator properties. The high specific capacities observed with the 130°C-CMC-PAA separator can be attributed to its favorable combination of wettability, porosity, and low interfacial resistance. The uniform pore distribution minimizes current hotspots and ensures homogeneous sodium ion flux. Additionally, the chemical compatibility between the separator and sodium-ion electrolyte reduces side reactions, as evidenced by the high Coulombic efficiency. Comparing with literature data, the CMC-PAA separators outperform many cellulose-based and modified polyolefin separators in terms of capacity retention and cycling stability for sodium-ion batteries.

Thermal stability is another advantage. The cross-linked ester bonds raise the decomposition onset temperature, allowing the separator to withstand operational heat generation without shrinking. This property is crucial for safety, especially in large-scale sodium-ion battery packs where thermal management is challenging. The dimensional integrity at elevated temperatures prevents internal short circuits, a common failure mode in batteries using conventional polyolefin separators.

From an environmental perspective, the use of water-soluble, biodegradable materials like CMC and PAA aligns with green chemistry principles. The fabrication process avoids toxic solvents, and the freeze-drying step is energy-efficient compared to supercritical drying. These aspects make the CMC-PAA aerogel separator a sustainable choice for next-generation sodium-ion batteries.

Conclusions and Future Perspectives

In this work, we developed and characterized novel aerogel separators for sodium-ion batteries using carboxymethyl cellulose sodium and polyacrylic acid. By varying the cross-linking temperature, we optimized the separator’s microstructure, mechanical properties, and electrochemical performance. The 130°C-CMC-PAA separator exhibited superior characteristics: high electrolyte uptake (>900%), low electrolyte leakage (0.42%), moderate ionic conductivity (1.877 mS/cm), excellent thermal stability up to 205 °C, and good flexibility (16.35% elongation at break). In sodium-ion half-cell tests, this separator delivered higher specific capacities and better cycling stability than commercial glass fiber separators across a wide range of current densities.

These findings underscore the potential of CMC-PAA aerogels as high-performance, eco-friendly separators for sodium-ion batteries. The tunable cross-linking approach allows precise control over pore structure, enabling customization for specific battery designs. Future research should explore several avenues to further advance this technology. First, investigating the effect of CMC-to-PAA ratio on separator properties could reveal additional optimization opportunities. Second, incorporating inorganic nanoparticles (e.g., SiO2, Al2O3) into the aerogel matrix may enhance mechanical strength and ionic conductivity. Third, long-term cycling tests in full sodium-ion battery cells are necessary to assess durability under realistic conditions. Fourth, scaling up the fabrication process using continuous freeze-drying or roll-to-roll methods would facilitate commercial adoption.

The development of advanced separators is pivotal for overcoming the current limitations of sodium-ion batteries, such as moderate energy density and cycle life. By improving separator performance, we can accelerate the deployment of sodium-ion batteries in applications ranging from stationary energy storage to electric vehicles. This study contributes to the growing body of knowledge on bio-based materials for energy storage, highlighting the synergy between sustainability and functionality. As research progresses, we anticipate that cellulose-derived aerogel separators will play a significant role in the future of sodium-ion battery technology, supporting the global transition to renewable energy.

Scroll to Top