The Case for Replacing the Liquid Electrolyte
Grid integration of wind and photovoltaic generation is limited less by installed capacity than by the temporal mismatch between output and demand. Because wind and solar output is intermittent and partly unpredictable, large-scale connection to the grid raises the burden of peak shaving and frequency regulation, and in several markets has led to curtailment of available generation. Storage is therefore the enabling component of any decarbonization pathway, including China’s stated targets of a carbon peak by 2030 and carbon neutrality by 2060.
Rechargeable lithium-ion batteries remain the most mature storage chemistry, but the cell itself carries an intrinsic hazard: the electrolyte is a volatile, flammable organic solvent system, and the porous separator that separates the electrodes offers no protection beyond mechanical shutdown. Thermal runaway, leakage, and internal short circuits are consequences of the liquid phase rather than of the lithium chemistry as such. A solid electrolyte addresses the problem at its origin — no combustible solvent, no separator, no leakage path, and a mechanical modulus high enough to resist penetration by lithium filaments. Because a solid electrolyte can also be paired with lithium metal or with high-capacity cathodes that are incompatible with liquid electrolytes, it opens a route to cell-level specific energies beyond the reach of conventional designs.
What an Ideal Solid Electrolyte Must Deliver
The requirements are demanding and partly conflicting:
- Lithium-ion conductivity above $10^{-3}\ \mathrm{S\,cm^{-1}}$ at room temperature;
- Electronic conductivity below $10^{-5}\ \mathrm{S\,cm^{-1}}$, so that the electrolyte does not internally short the cell;
- An electrochemical window wide enough to contact both a low-potential anode and a high-potential cathode;
- Chemical and electrochemical compatibility with both electrodes, with low interfacial resistance;
- Sufficient shear modulus to suppress lithium dendrite penetration;
- Non-toxicity, non-flammability, and thermal stability;
- Low raw-material cost and a scalable fabrication route.
No single material satisfies all of these. Liquid electrolytes conduct superbly but fail the safety and mechanical criteria; polymer electrolytes are flexible and easy to process but conduct poorly at ambient temperature; inorganic electrolytes offer high transference numbers and thermal stability but are brittle and form poor interfaces. This trade-off, rather than any single materials gap, defines the current research agenda.
Inorganic Solid Electrolytes
Inorganic solid electrolytes fall into four structural families of practical interest — LISICON, NASICON, perovskite, and garnet — plus the sulfide glasses and the oxynitrides, which are better classified by anion chemistry. They can also be grouped simply as oxides, sulfides, and nitrides, a division that maps closely onto their stability and processing behavior.
LISICON Frameworks and the Sulfide Superionic Conductors
The LISICON (lithium superionic conductor) family derives from the compound $\mathrm{Li_{14}Zn(GeO_4)_4}$, synthesized by H. Y.-P. Hong and co-workers, which reaches $0.13\ \mathrm{S\,cm^{-1}}$ at 300 °C. Single-crystal X-ray analysis gives lattice parameters $a = 10.828\ \text{Å}$, $b = 6.251\ \text{Å}$, and $c = 5.140\ \text{Å}$, with a rigid three-dimensional $[\mathrm{Li_{11}Zn(GeO_4)_4}]^{3-}$ framework built from $[\mathrm{GeO_4}]^{2-}$ tetrahedra; it can be regarded as a solid solution of $\mathrm{Li_4GeO_4}$ and $\mathrm{Zn_2GeO_4}$. Lithium ions migrate through vacancies and interstitial sites of this skeleton.
Structurally, the family descends from $\gamma\text{-}\mathrm{Li_3PO_4}$, in which Li and P occupy half of the tetrahedral sites of a distorted hexagonal close-packed array. Aliovalent substitution on the phosphorus site requires additional lithium for charge compensation, and those extra ions sit in interstitial octahedral positions. For $\mathrm{Li_4MO_4}$-type hosts ($M = \mathrm{Si}$, $\mathrm{Ge}$, $\mathrm{Ti}$), supervalent substitution yields compositions of the form $\mathrm{Li_{4-y}M_xN_{1-x}O_4}$, where three lithium ions belong to the tetrahedral framework and the remaining $1-y$ per formula unit are interstitial, with
$$y = \left[x\,n_1 + (1-x)\,n_2\right] – 4,$$
where $n_1$ and $n_2$ are the charges of the $M^{n_1+}$ and $N^{n_2+}$ cations.
Oxide conductivity in this family is modest, and the standard remedy is anion substitution: replacing $\mathrm{O^{2-}}$ with the larger, less polarizing $\mathrm{S^{2-}}$ widens the lithium migration channels and raises conductivity, at the cost of chemical stability. This logic culminated in 2011 with $\mathrm{Li_{10}GeP_2S_{12}}$ (LGPS), reported by N. Kamaya and co-workers and prepared by high-temperature solid-state reaction, which reaches $1.2\times10^{-2}\ \mathrm{S\,cm^{-1}}$. A $\mathrm{LiCoO_2/LGPS/Li}$ cell delivered initial discharge and charge capacities of 135 and $124\ \mathrm{mA\,h\,g^{-1}}$ at $14\ \mathrm{mA\,g^{-1}}$, a Coulombic efficiency of 91.85%.
In 2016, Y. Kato and co-workers introduced Si and Cl into the LGPS framework to obtain $\mathrm{Li_{9.54}Si_{1.74}P_{1.44}S_{11.7}Cl_{0.3}}$, with a room-temperature conductivity of $2.5\times10^{-2}\ \mathrm{S\,cm^{-1}}$ — twice that of LGPS — and lower raw-material cost. Cells built with this conductor operated at 18C and over $-30$ to 100 °C, performance that the authors placed above contemporary liquid-electrolyte cells. The weakness of the whole sulfide branch remains chemical: limited intrinsic stability against lithium and against oxide cathodes, side reactions, dendrite growth, and interfacial mechanical failure.
NASICON
The sodium superionic conductor concept was introduced in 1976 by John B. Goodenough and co-workers, who reported $\mathrm{Na_{1+x}Zr_2Si_xP_{3-x}O_{12}}$, a framework structurally related to $\beta\text{-}\mathrm{Al_2O_3}$. At $x = 2$ the material reached $5\ \mathrm{S\,cm^{-1}}$ at 300 °C, the highest reported for a sodium conductor at the time; lithium analogues followed. The best-known lithium members, $\mathrm{Li_{1.3}Al_{0.3}Ti_{1.7}(PO_4)_3}$ (LATP) and $\mathrm{Li_{1.5}Al_{0.5}Ge_{1.5}(PO_4)_3}$ (LAGP), exceed $10^{-3}\ \mathrm{S\,cm^{-1}}$, but the $\mathrm{Ti^{4+}}$ and $\mathrm{Ge^{4+}}$ centers are readily reduced on contact with lithium metal, which restricts their use to cathodes or to protected configurations. Stability against lithium therefore tracks the presence of reducible transition metals: $\mathrm{LiM(PO_4)_3}$ with $M = \mathrm{Zr}$, $\mathrm{Sc}$, $\mathrm{Hf}$ is comparatively robust. $\mathrm{LiZr(PO_4)_3}$ (LZP) is cheap but conducts only about $10^{-8}\ \mathrm{S\,cm^{-1}}$; cation doping raises this by roughly two orders of magnitude, and calcium substitution at the zirconium site, giving $\mathrm{Li_{1.2}Zr_{1.9}Ca_{0.1}(PO_4)_3}$, converts the triclinic phase into a stable orthorhombic one and reaches $1.2\times10^{-4}\ \mathrm{S\,cm^{-1}}$ at 25 °C.
Perovskite Titanates
Y. Inaguma and co-workers first prepared the perovskite-type conductor $\mathrm{Li_{3x}La_{2/3-x}TiO_3}$ (LLTO); $\mathrm{Li_{0.34}La_{0.51}TiO_{2.94}}$ shows a bulk conductivity of $1\times10^{-3}\ \mathrm{S\,cm^{-1}}$ at room temperature but a total conductivity above only $2\times10^{-5}\ \mathrm{S\,cm^{-1}}$, the difference being the grain-boundary contribution. In the $\mathrm{ABO_3}$ framework, Li and La share the twelve-coordinate A site while Ti occupies the six-coordinate B site; oxygen ions form bottlenecks between neighboring A sites, so the lattice parameter controls the migration barrier. Doping 5% $\mathrm{Sr^{2+}}$ onto the A site of $\mathrm{Li_{1/2}La_{1/2}TiO_3}$ expands the lattice and gives $1.5\times10^{-3}\ \mathrm{S\,cm^{-1}}$ at 27 °C, but higher Sr content depletes the lithium concentration and conductivity falls again.
The more serious limitation is electrochemical. LLTO is unstable below about 1.8 V versus $\mathrm{Li/Li^+}$, because $\mathrm{Ti^{4+}}$ is reduced at potentials where lithium plating occurs, introducing electronic conductivity and interfacial degradation. Lithium insertion into $\mathrm{Li_{0.35}La_{0.55}TiO_3}$ proceeds in two stages, 1.8–1.1 V and 0.6–0 V; the first step inserts 0.75–0.9 Li per formula unit, but only 0.48 is reversibly extracted, and at a doping level of 0.24 Li the perovskite transforms toward a monoclinic $\mathrm{A_2BO_3}$ phase. Substitution of titanium is therefore necessary for stability, and poor contact with electrode materials adds a further interfacial resistance that has so far blocked commercialization.
Garnet
Garnets follow the general formula $\mathrm{A_3B_2(XO_4)_3}$, as in $\mathrm{Ca_3Al_2(SiO_4)_3}$ (cubic, space group $Ia\bar{3}d$, No. 230), where A, B, and X are eight-, six-, and four-coordinate cations and $[\mathrm{XO_4}]$ tetrahedra are linked through B–O bonds. Lithium garnets are obtained by placing lithium on the X site; doping the A or B site then tunes the lithium content, the vacancy concentration, and the cell parameters. Two phases exist under the same framework — tetragonal, in which the tetrahedral, octahedral, and distorted octahedral sites are fully occupied, and cubic, in which lithium is disordered — and the different diffusion mechanism gives the cubic phase a conductivity roughly two orders of magnitude higher.
In 2003, V. Thangadurai and co-workers reported $\mathrm{Li_5La_3M_2O_{12}}$ ($M = \mathrm{Ta}$, $\mathrm{Nb}$) with a conductivity near $10^{-5}\ \mathrm{S\,cm^{-1}}$ at room temperature and good chemical stability over a wide temperature range. In 2007, R. Murugan and co-workers reported $\mathrm{Li_7La_3Zr_2O_{12}}$ (LLZO), which reaches the $10^{-4}\ \mathrm{S\,cm^{-1}}$ range at 25 °C in the cubic phase. Doping remains the standard route both to stabilize the cubic phase and to raise conductivity: germanium doping below 1 wt% gives $8.3\times10^{-4}\ \mathrm{S\,cm^{-1}}$ at room temperature, and gallium doping in $\mathrm{Li_{7-3x}Ga_xLa_3Zr_2O_{12}}$ with $x = 0.25$ gives $1.46\times10^{-3}\ \mathrm{S\,cm^{-1}}$ at 25 °C. The wide window of about 6 V versus $\mathrm{Li/Li^+}$ and the relative stability of garnets against both lithium metal and typical oxide cathodes make them attractive for high-voltage cells. The practical difficulties are interfacial: poor wetting by lithium, dendrite growth inside the ceramic, and side reactions at the lithium interface.
Sulfide Glasses and Glass-Ceramics
In the $\mathrm{Li_2S\text{-}P_2S_5}$ system, several crystalline phases are known — $\mathrm{Li_2P_2S_6}$ (50:50), $\mathrm{Li_7P_3S_{11}}$ (70:30), $\mathrm{Li_3PS_4}$ (75:25), $\mathrm{Li_7PS_6}$ (88:12), and $\mathrm{Li_4P_2S_6}$ (67:33) — and the phase that forms depends on glass composition and heat treatment. Crystallization usually lowers conductivity, because the individual crystalline phases conduct less than the glass. Compositions richer in $\mathrm{Li_2S}$ ($x \geq 70$) contain more isolated $\mathrm{PS_4^{3-}}$ tetrahedra with fully terminal sulfur; the 75:25 glass, in which every sulfur is terminal, reaches $2.8\times10^{-4}\ \mathrm{S\,cm^{-1}}$ at room temperature. Related binaries such as $x\mathrm{Li_2S}\cdot(100-x)\mathrm{B_2S_3}$ and $x\mathrm{Li_2S}\cdot(100-x)\mathrm{SiS_2}$ conduct near $10^{-4}\ \mathrm{S\,cm^{-1}}$ over wide composition ranges.
Doping is the standard means of raising carrier concentration. Addition of $\mathrm{Li_3PO_4}$, $\mathrm{Li_4SiO_4}$, or $\mathrm{Li_4GeO_4}$ to $x\mathrm{Li_2S}\cdot(100-x)\mathrm{SiS_2}$ pushes conductivity above $10^{-3}\ \mathrm{S\,cm^{-1}}$ while retaining a wide electrochemical window; $\mathrm{LiBO_3}$ and $\mathrm{LiAlO_3}$ improve thermal stability and resistance to crystallization at comparable conductivity. Lithium borohydride acts as an effective dopant: $77(75\mathrm{Li_2S}\cdot25\mathrm{P_2S_5})\cdot33\mathrm{LiBH_4}$ reaches $1.6\times10^{-3}\ \mathrm{S\,cm^{-1}}$ and is stable to 5 V versus $\mathrm{Li/Li^+}$. Lithium halides work similarly — $30\mathrm{Li_2S}\cdot26\mathrm{B_2S_3}\cdot33\mathrm{LiI}$ gives $1.7\times10^{-3}\ \mathrm{S\,cm^{-1}}$, and $40\mathrm{Li_2S}\cdot28\mathrm{SiS_2}\cdot30\mathrm{LiI}$ gives $1.8\times10^{-3}\ \mathrm{S\,cm^{-1}}$ at room temperature.
The unresolved problem is hydrolytic. Sulfides react with ambient moisture to release hydrogen sulfide, with the characteristic odor of rotten eggs, while the structure degrades and conductivity falls. This handling constraint, rather than any transport limitation, is the principal obstacle to commercial deployment.
Oxynitride Thin Films
Lithium phosphorus oxynitride (LiPON) was first reported by J. Bates and co-workers, who sputtered a $\mathrm{Li_3PO_4}$ target in nitrogen to obtain an amorphous film of composition $\mathrm{Li_{2.9}PO_{3.3}N_{0.46}}$ with a room-temperature conductivity of $3.3\times10^{-6}\ \mathrm{S\,cm^{-1}}$, an activation energy of 0.54 eV, and an operating window of 5.5 V versus $\mathrm{Li/Li^+}$. Y. Hamon and co-workers later deposited $\mathrm{Li_{3.0}PO_{2.0}N_{1.2}}$ by magnetron sputtering in pure nitrogen and showed that raising the nitrogen content of the glass network markedly increases conductivity. LiPON conducts poorly compared with the crystalline families and is not stable against lithium metal, but it has enabled a commercial product: thin-film microbatteries that sustain tens of thousands of cycles.
Polymer Electrolytes
Polymer electrolytes offer high interfacial compatibility and simple, roll-to-roll compatible processing, and are therefore attractive for volume manufacturing. Their limitation is transport: most host polymers are semicrystalline, and lithium conduction occurs predominantly in the amorphous phase, so intrinsic conductivities generally fall below $10^{-6}\ \mathrm{S\,cm^{-1}}$ at room temperature.
Poly(ethylene oxide)
The dissociation and transport of salts in poly(ethylene oxide) (PEO) was studied in 1981 by F. L. Tanzella and co-workers, who prepared and characterized complexes of PEO with $\mathrm{LiCF_3COO}$, NaSCN, and KSCN. Conductivity appeared only below the melting point of each complex — 115 °C for $(\mathrm{PEO})_5\mathrm{LiCF_3COO}$, 120 °C for the KSCN complex, and 195 °C for the NaSCN complex — with hydrated films conducting better than dry ones, and solid-state NMR on blocking and non-blocking electrodes identified lithium as the principal mobile species. PEO remains the most widely used polymer host: conduction proceeds by coordination of lithium to the lone pairs of the ether oxygen, with repeated formation and breaking of those bonds along the chain.
Because crystalline domains block transport, conductivity is low at ambient temperature and rises sharply above the melting range of 50–80 °C, where values near $10^{-3}\ \mathrm{S\,cm^{-1}}$ can be reached. Excessive amorphization, conversely, degrades mechanical strength, and the amorphous phase is metastable and may crystallize over time, lowering both conductivity and transference number. Crosslinking and interpenetration are the usual countermeasures: a polyacrylonitrile–PEO interpenetrating crosslinked gel membrane reported by P.-L. Kuo and co-workers in 2014 reached 1.06–8.21 mS cm⁻¹, retained more than 97% Coulombic efficiency after 100 cycles at 1C, and outperformed commercial separators across 0.1–3C.
Polycarbonates
Aliphatic polycarbonates carry highly polar carbonate groups whose oxygen atoms withdraw lone-pair density only weakly, so the coordination bond formed with lithium is weaker and ion hopping between coordination sites is easier — the origin of their higher conductivity. In 2015, K. Kimura and co-workers built a $\mathrm{PEC\text{-}LiTFSI\text{-}Pyr_{14}TFSI}$ composite on a poly(ethylene carbonate) (PEC) base using nanoscale silica fiber as an inert filler; the low glass transition and plasticizing action of the ionic liquid raised both conductivity and mechanical strength. The material conducted at $10^{-5}\ \mathrm{S\,cm^{-1}}$ at 80 °C and operated in a $\mathrm{Li/LiFePO_4}$ prototype delivering about $100\ \mathrm{mA\,h\,g^{-1}}$ at C/15 and 75 °C. A poly(propylene carbonate) electrolyte plasticized with the ionic liquid VIm-TFSI reached $8.2\times10^{-5}\ \mathrm{S\,cm^{-1}}$ at room temperature while supporting reversible lithium plating and stripping, improving rate capability and cycling of $\mathrm{LiFePO_4\text{-}Li}$ cells.
Poly(vinylene carbonate) (PVCA) illustrates the mechanical advantage of a rigid cyclic carbonate backbone. The PVCA-based gel electrolyte reported by J. Chai and co-workers in 2017 conducts at $5.59\times10^{-4}\ \mathrm{S\,cm^{-1}}$, has a window above 4.8 V at ambient temperature, and in a $\mathrm{LiFe_{0.2}Mn_{0.8}PO_4/graphite}$ full cell retained 88.7% of capacity after 1 000 cycles at 1C while delivering $90\ \mathrm{mA\,h\,g^{-1}}$ at 8C. Relative to PEO, polycarbonate systems tolerate a wider temperature range, but the lithium transport mechanism within them is still incompletely characterized and a scalable manufacturing route has yet to be established.
Other Matrices
Poly(vinylidene fluoride) and its hexafluoropropylene copolymer, polyacrylonitrile, and polyimide are also used, generally not as conductors but as mechanically and thermally robust scaffolds that are combined with a lithium-conducting phase.
Composite Electrolytes
Neither inorganic nor polymer electrolytes alone meet the industrialization requirements: ceramics fail on interfaces and processability, polymers on conductivity. Dispersing an inorganic phase in a polymer matrix combines the two, and composition can be tuned to trade one property against another. The inorganic component is either an active filler that participates in lithium transport or an inert filler that does not.
Inert Fillers
The effect of inert fillers was already visible in 1973, when C. C. Liang added $\mathrm{Al_2O_3}$ to polycrystalline LiI and observed a conductivity increase without any chemical reaction — an observation classical doping theory could not explain. J. Maier proposed a space-charge mechanism in 1985, in which interfacial interaction between the two phases modifies ionic conductance. Fillers such as $\mathrm{Al_2O_3}$, $\mathrm{SiO_2}$, $\mathrm{TiO_2}$, $\mathrm{ZrO_2}$, $\mathrm{Fe_2O_3}$, and $\mathrm{B_2O_3}$, especially at the nanoscale, raise conductivity by disrupting polymer chain crystallization and enlarging the amorphous fraction; surface groups also promote lithium salt dissociation, increasing the population of free $\mathrm{Li^+}$, while Lewis acid–base interaction with the anion weakens the polymer–cation complexation that otherwise traps lithium. Carbon nanotubes, graphene, and metal–organic frameworks act similarly by creating additional or lower-energy conduction pathways.
A clear example is the $\mathrm{PEO\text{-}LiTFSI\text{-}Mg_2B_2O_5}$ system reported by O. Sheng and co-workers in 2018, in which $\mathrm{Mg^{2+}}$ on the nanowire surface interacts with $\mathrm{TFSI^-}$, weakening the $\mathrm{Li^+\text{-}TFSI^-}$ association and releasing more free lithium. Paired with $\mathrm{LiFePO_4}$, the electrolyte delivered 150, 106, and $50\ \mathrm{mA\,h\,g^{-1}}$ at 0.2C at 50, 40, and 30 °C respectively.
Active Fillers
Active fillers conduct lithium themselves, so their intrinsic conductivity strongly influences the composite. Most inorganic solid electrolytes can serve this role. In 2019, Y. Wang and co-workers fabricated a vertically aligned $\mathrm{LAGP/PEO}$ composite in which the ceramic provides continuous fast channels and the polymer supplies flexibility; conductivity was $1.67\times10^{-4}\ \mathrm{S\,cm^{-1}}$ at room temperature and $1.11\times10^{-3}\ \mathrm{S\,cm^{-1}}$ at 60 °C, and a $\mathrm{LiFePO_4/LAGP\text{-}PEO/Li}$ cell retained 93.3% of capacity after 300 cycles. Because polycrystalline fillers contribute their own grain-boundary resistance, the net gain in composite conductivity is often modest, and it remains unclear whether combining two active conductors creates new percolating paths or merely preserves the two conduction networks in parallel.
Comparative Picture
| Family | Representative | Room-temperature $\sigma_{\mathrm{Li^+}}$ | Principal strength | Principal limitation |
|---|---|---|---|---|
| LISICON oxide | $\mathrm{Li_{14}Zn(GeO_4)_4}$ | $0.13\ \mathrm{S\,cm^{-1}}$ at 300 °C | Thermal and electrochemical stability | Low ambient conductivity; unstable against Li |
| NASICON | LATP, LAGP, LZP | above $10^{-3}\ \mathrm{S\,cm^{-1}}$ (LATP, LAGP) | Air stability; wide composition space | $\mathrm{Ti^{4+}}$, $\mathrm{Ge^{4+}}$ reduced by lithium metal |
| Perovskite | $\mathrm{Li_{3x}La_{2/3-x}TiO_3}$ | bulk $10^{-3}$, total $\sim10^{-5}\ \mathrm{S\,cm^{-1}}$ | High bulk conductivity | Grain-boundary resistance; unstable below 1.8 V |
| Garnet | $\mathrm{Li_7La_3Zr_2O_{12}}$ | $10^{-4}$ (cubic, undoped); $1.46\times10^{-3}$ (Ga-doped) | Window near 6 V; stable against Li | Poor wetting; dendrites inside ceramic |
| Sulfide | LGPS; $\mathrm{Li_{9.54}Si_{1.74}P_{1.44}S_{11.7}Cl_{0.3}}$ | $1.2\times10^{-2}$; $2.5\times10^{-2}\ \mathrm{S\,cm^{-1}}$ | Highest conductivity; ductility | Hydrolyzes to $\mathrm{H_2S}$; narrow stability window |
| Oxynitride | LiPON | $3.3\times10^{-6}\ \mathrm{S\,cm^{-1}}$ | Thin-film processing; 5.5 V window | Low conductivity; vacuum deposition cost |
| Polymer | PEO, PEC, PVCA | $10^{-6}$ to $10^{-4}\ \mathrm{S\,cm^{-1}}$ | Flexibility; scalable coating | Low ambient conductivity; oxidation limit |
| Composite | $\mathrm{LAGP/PEO}$; $\mathrm{PEO\text{-}Mg_2B_2O_5}$ | $1.67\times10^{-4}\ \mathrm{S\,cm^{-1}}$ (aligned LAGP/PEO) | Balanced properties; tunable | Percolation control; filler dispersion |
Industrialization
National strategies diverge by materials preference. European and North American developers place safety first and favor oxide and polymer systems, which are the most stable; Japanese and Korean firms concentrate on sulfides, seeking to retain the high-capacity advantage while correcting the stability defects. Chinese activity has prioritized initial capacity and driving range, and although it started later than in Germany, the United States, and Japan, the participant base now spans research institutes (the Institute of Chemistry and the Qingdao Institute of Bioenergy and Bioprocess Technology of the Chinese Academy of Sciences, the Ningbo Institute of Materials Technology and Engineering), battery manufacturers such as Ganfeng Lithium and CATL, and cross-sector investors including the automotive supplier Wanxiang and BYD.
Policy has reinforced the direction. In October 2020 the State Council issued the New Energy Vehicle Industry Development Plan (2021–2035), emphasizing research and industrialization of solid-state power batteries. The China Society of Automotive Engineers’ Technology Roadmap 2.0 for energy-saving and new energy vehicles set specific-energy targets for high-energy cells of 350 Wh kg⁻¹ by 2025, 400 Wh kg⁻¹ by 2030, and 500 Wh kg⁻¹ by 2035.
| Developer | Electrolyte route | Disclosed performance | Status reported |
|---|---|---|---|
| ProLogium | Mixed oxide, solid–liquid hybrid | $\mathrm{SiO_x}$/graphite cells: 440–485 Wh L⁻¹, over 1 000 cycles, 5C charging; lithium-metal prototype: 383 Wh kg⁻¹ and 1 025 Wh L⁻¹ over 500 cycles | Pilot production 2023; volume production from 2024 |
| QingTao Energy | Mixed oxide, solid–liquid hybrid | Discharge capacity above 116 Ah at 1/3C; 368 Wh kg⁻¹ | First production line 2018; national certification September 2021; 10 GWh base under construction with RMB 5.5 billion investment |
| WeLion New Energy | Mixed oxide, in-situ curing | Above 300 Wh kg⁻¹ (2018); 360 Wh kg⁻¹ hybrid cells, 1 000 km vehicle range | 2 GWh line; ~20 GWh targeted by 2026; 400 Wh kg⁻¹ targeted for 2025 and 600 Wh kg⁻¹ for 2030 |
Two routes dominate among Chinese manufacturers: all-solid-state cells based on sulfide electrolytes, and hybrid cells that retain a small liquid fraction. The liquid component relaxes the interfacial contact problem between rigid electrolyte and rigid electrode, at some cost in thermal stability, and — decisively — allows existing lithium-ion production equipment to be reused. Given material and equipment constraints, hybrid designs are the nearer-term path and are close to volume production. The performance figures above come from company disclosures and public statements, and are subject to revision.
Open Problems
Laboratory-scale cells are far from a manufacturable product. Several bottlenecks remain unresolved: low-cost, high-throughput production of electrolyte material; fabrication of thin free-standing membranes that combine mechanical strength with ionic conduction; high cathode loading and utilization; and stable, low-resistance contact between electrolyte and electrode. Pouch-cell configuration and assembly introduce further constraints. Operation adds its own failure modes — gas evolution, interfacial side reactions, and progressive loss of contact during cycling — that existing diagnostic techniques were not designed to resolve, so failure-analysis methods specific to solid-state cells are needed. Closing these gaps requires coordination across the whole battery supply chain rather than advances in a single material.