Dynamic Modeling and Control of Lithium Ion Battery Winding Stress

I have long been interested in the manufacturing mechanics of lithium ion battery cells because the winding step is one of the most influential stages in determining the safety, consistency, and electrochemical performance of cylindrical lithium ion battery products. In a high-speed winding machine, the positive electrode, the negative electrode, and the two separator layers are wound together onto a rotating mandrel. During this process, the web materials are subjected to tension, and the accumulated layers generate internal stress. If the internal stress becomes too high, the electrode or separator may deform, wrinkle, or even fracture. If the internal stress becomes too low, the layers may become loose and form folds. Both conditions are unacceptable for a high-quality lithium ion battery cell. I therefore constructed a dynamic model of the internal stress in the wound cell, analyzed several tension control strategies, and validated the selected control scheme through experiments on a high-speed winding platform.

1. Introduction

A lithium ion battery offers high energy density, good cycling stability, a high safety factor, a long service life, a low self-discharge rate, and fast charging capability. These advantages have made the lithium ion battery a preferred power source in electric vehicles, aerospace systems, portable electronics, and office equipment. In a cylindrical lithium ion battery, the cell is produced by winding a positive electrode, a first separator, a negative electrode, and a second separator into a cylindrical roll. The winding process is therefore not merely a geometric shaping operation; it is a coupled mechanical process in which web tension, friction, inertia, and layer interaction determine the final internal state of the lithium ion battery cell.

During high-speed winding, the web materials are pulled at speeds greater than 3 m/s. At such speeds, the inertial force of the rotating web cannot be ignored. The internal stress in the wound lithium ion battery cell is influenced by the winding radius, the winding speed, the elastic properties of the electrodes and separator, the mandrel radius, the web thickness, and the tension profile. A poor tension profile can cause the positive electrode, negative electrode, or separator to exceed its elastic limit. It can also cause the inner layers to lose tension and form wrinkles. Wrinkles and folds may create local short circuits, which are a serious safety concern for any lithium ion battery. Therefore, I focused on the dynamic modeling of internal stress and on the selection of a suitable tension control method for high-speed winding of lithium ion battery cells.

Previous studies have examined internal stress in wound cells and have proposed constant tension, tapered tension, parabolic tension, and composite tension profiles. Some researchers have studied the fracture of current collectors, the deformation of pouch cells, and the effect of taper tension on telescoping. However, many of these studies do not explicitly include the high-speed condition. For a lithium ion battery cell made of thin, compliant, and layered materials, the winding speed strongly affects the centrifugal force and the resulting stress state. I therefore developed a dynamic model that includes the winding speed, the mandrel radius, the web thickness, and the tension profile. Using this model, I compared constant tension winding and tapered tension winding, and I selected a constant tension scheme for a cylindrical lithium ion battery cell. The experimental results confirmed that the proposed scheme maintains tension fluctuation within the required range and produces a lithium ion battery cell with acceptable height and diameter.

2. Mechanical Model of the Winding Process

2.1 Assumptions

I treated the wound assembly as a layered continuum and simplified the problem as an axisymmetric plane strain problem. The positive electrode, the first separator, the negative electrode, and the second separator were considered as a single effective web for the macroscopic stress analysis. The mandrel was treated as a rigid body. The material was assumed to be macroscopically homogeneous and isotropic in the plane of the web. The winding speed was assumed to be constant at a given operating point, and the tension was assumed to be applied uniformly across the web width. The main assumptions are summarized in Table 1.

Assumption Description
Geometry Axisymmetric cylindrical roll
Strain state Plane strain in the axial direction
Material behavior Linear elastic, macroscopically homogeneous
Mandrel Rigid, circular, no radial displacement
Web layers Thin, perfectly bonded, no slip between layers
Winding speed Constant high speed, inertial force included
Tension Uniform across web width

2.2 Equilibrium and Constitutive Relations

For a cylindrical roll under axisymmetric loading, the radial equilibrium equation can be written as

$$ \frac{d\sigma_r}{dr}+\frac{\sigma_r-\sigma_\theta}{r}+f_r=0 $$

where \( \sigma_r \) is the radial stress, \( \sigma_\theta \) is the tangential stress, \( r \) is the radial coordinate, and \( f_r \) is the inertial body force per unit volume. The inertial force arises from the rotation of the lithium ion battery web material and is given by

$$ f_r=\rho \omega^2 r=\rho \frac{V^2}{r} $$

where \( \rho \) is the effective density of the wound lithium ion battery materials, \( \omega \) is the angular velocity, and \( V \) is the winding line speed. I used the plane strain constitutive relations

$$ \varepsilon_\theta=\frac{1}{E_\theta}\left(\sigma_\theta-\nu\sigma_r\right) $$

$$ \varepsilon_r=\frac{1}{E_r}\left(\sigma_r-\nu\sigma_\theta\right) $$

where \( \varepsilon_r \) and \( \varepsilon_\theta \) are the radial and tangential strains, \( E_r \) and \( E_\theta \) are the radial and tangential elastic moduli, and \( \nu \) is the Poisson ratio. The radial displacement \( u \) is related to the tangential strain by

$$ \varepsilon_\theta=\frac{u}{r} $$

Solving the equilibrium equation with the inertial term yields the general stress distributions

$$ \sigma_r=C_1+C_2 r $$

$$ \sigma_\theta=C_1+2C_2 r+\rho V^2 $$

where \( C_1 \) and \( C_2 \) are constants determined by the boundary conditions. Substituting these stress expressions into the constitutive relations gives

$$ \varepsilon_r=\frac{1}{E_r}\left[(1-\nu)C_1+(1-2\nu)C_2 r-\nu\rho V^2\right] $$

$$ \varepsilon_\theta=\frac{1}{E_\theta}\left[(1-\nu)C_1+(1-2\nu)C_2 r-\rho V^2\right] $$

The radial displacement is therefore

$$ u=\frac{r}{E_\theta}\left[(1-\nu)C_1+(1-2\nu)C_2 r+\rho V^2\right] $$

2.3 Boundary Conditions

I assumed that the mandrel is rigid and that no radial displacement occurs at the mandrel surface. At the outer surface of the roll, the radial stress is equal to the negative of the contact pressure \( p \). Therefore, the boundary conditions are

$$ u\big|_{r=R_0}=0,\qquad \sigma_r\big|_{r=R}=-p $$

where \( R_0 \) is the mandrel radius and \( R \) is the current outer radius of the wound lithium ion battery cell. Substituting the boundary conditions into the general solutions gives

$$ \frac{R_0}{E_\theta}\left[(1-\nu)C_1+(2-\nu)C_2 R_0+\rho V^2\right]=0 $$

$$ C_1+C_2 R=-p $$

Solving these equations for \( C_1 \) and \( C_2 \) and substituting back yields the radial stress

$$ \sigma_r=-\frac{\rho V^2 R+p(2-\nu)R_0}{(1-\nu)R+(2-\nu)R_0}+\frac{\rho V^2-p(1-\nu)}{(1-\nu)R+(2-\nu)R_0}r $$

and the tangential stress

$$ \sigma_\theta=-\frac{\rho V^2 R+p(2-\nu)R_0}{(1-\nu)R+(2-\nu)R_0}+\frac{2r\left[\rho V^2-p(1-\nu)\right]}{(1-\nu)R+(2-\nu)R_0}+\rho V^2 $$

The corresponding strains are

$$ \varepsilon_r=\frac{1}{E_r}\left[(\nu-1)\frac{\rho V^2 R+p(2-\nu)R_0}{(1-\nu)R+(2-\nu)R_0}+(1-2\nu)r\frac{\rho V^2-p(1-\nu)}{(1-\nu)R+(2-\nu)R_0}-\nu\rho V^2\right] $$

$$ \varepsilon_\theta=\frac{r}{E_\theta}\left[(\nu-1)\frac{\rho V^2 R+p(2-\nu)R_0}{(1-\nu)R+(2-\nu)R_0}+(2-\nu)r\frac{\rho V^2-p(1-\nu)}{(1-\nu)R+(2-\nu)R_0}+\rho V^2\right] $$

These expressions show that both the radial and tangential stresses depend on the current outer radius \( R \), the radial coordinate \( r \), the winding speed \( V \), the contact pressure \( p \), and the elastic properties of the lithium ion battery web materials.

2.4 Contact Pressure and Layer Interaction

When the lithium ion battery cell is wound to the \( j \)-th layer, the outer radius is \( R_j \), and the winding tension is \( F_T(R_j) \). The tensile stress on the cross section of the \( j \)-th layer is

$$ \sigma(R_j)=\frac{F_T(R_j)}{S} $$

where \( S \) is the cross-sectional area of the web. The pressure exerted on the inner layers by the \( j \)-th layer can be approximated as

$$ p=\frac{\sigma(R_j)T}{R_j-T} $$

where \( T \) is the web thickness. Because the thickness of the positive electrode, negative electrode, and separator is very small compared with the wound radius, I neglected \( T \) in the denominator and obtained

$$ p=\frac{\sigma(R_j)T}{R_j-T}\approx\frac{F_T(R_j)}{R_j b} $$

where \( b \) is the web width. At the outer surface of the roll, the tangential stress must equal the winding tensile stress. Therefore,

$$ \sigma_\theta(r,R)\big|_{r=R}=\sigma_\theta(R,R)=\frac{F_T(R)}{S} $$

This boundary condition links the macroscopic tension applied by the winding machine to the internal stress field of the lithium ion battery cell.

2.5 Accumulated Tangential Stress Model

As winding continues, every new layer adds stress to all existing layers. I considered a point at radius \( r \) in the \( i \)-th layer. When the outer radius increases from \( R_i \) to the final radius \( R_n \), the tangential stress at that point is the sum of the direct winding stress and the contributions from all subsequent layers. Thus,

$$ \sigma_\theta(r,R_n)=\frac{F_T(r)}{S}+\frac{1}{T}\left\{\sum_{k=i}^{n}\left[\sigma_\theta(r,R_k)\Delta R_k\right]\right\} $$

Because the web thickness is very small and the number of layers is large, I replaced the summation with an integral. Combining the stress expressions with the contact pressure relation gives the accumulated tangential stress in the final lithium ion battery cell:

$$ \sigma_\theta(r,R_n)=\frac{F_T(r)}{S}+\left[\frac{\rho V^2(2-\nu)R_0}{(1-\nu)^2T}-\frac{F_T(R)}{bT}+\frac{2r\rho V^2}{(1-\nu)T}+\frac{2rF_T(R)(1-\nu)}{T(2-\nu)R_0 b}\right]\ln\left(\frac{(1-\nu)R_n+(2-\nu)R_0}{(1-\nu)r+(2-\nu)R_0}\right)-\frac{\rho V^2(R_n-r)\nu}{(1-\nu)T} $$

Similarly, the accumulated radial stress is

$$ \sigma_r(r,R_n)=\left[\frac{\rho V^2(2-\nu)R_0}{(1-\nu)^2T}-\frac{F_T(R)}{bT}+\frac{r\rho V^2}{(1-\nu)T}+\frac{rF_T(R)(1-\nu)}{T(2-\nu)R_0 b}\right]\ln\left(\frac{(1-\nu)R_n+(2-\nu)R_0}{(1-\nu)r+(2-\nu)R_0}\right)-\frac{\rho V^2(R_n-r)}{(1-\nu)T} $$

These equations form the core of the dynamic model. They describe how the internal stress in a lithium ion battery cell evolves with winding radius, winding speed, tension, material properties, and mandrel radius. Table 2 lists the main variables and their meanings.

Symbol Meaning Unit
\( \sigma_r \) Radial stress Pa
\( \sigma_\theta \) Tangential stress Pa
\( \varepsilon_r \) Radial strain –
\( \varepsilon_\theta \) Tangential strain –
\( r \) Radial coordinate m
\( R \) Current outer radius m
\( R_0 \) Mandrel radius m
\( R_n \) Final outer radius m
\( T \) Web thickness m
\( b \) Web width m
\( V \) Winding line speed m/s
\( \rho \) Effective density kg/m\(^3\)
\( \nu \) Poisson ratio –
\( E_r \) Radial elastic modulus Pa
\( E_\theta \) Tangential elastic modulus Pa
\( F_T \) Winding tension N
\( p \) Contact pressure Pa
\( \Psi \) Taper tension coefficient –

3. Tension Control Strategies

The tension profile determines the internal stress distribution in the lithium ion battery cell. I examined two widely used strategies: constant tension winding and tapered tension winding. In constant tension winding, the tension is kept constant throughout the entire winding process:

$$ F_T(R)=F_{T0} $$

In tapered tension winding, the tension decreases linearly as the outer radius increases:

$$ F_T(R)=F_{T0}-\Psi F_{T0}\frac{R}{R_0} $$

where \( F_{T0} \) is the initial tension and \( \Psi \) is the taper coefficient. When \( \Psi=0 \), the tapered tension law reduces to constant tension. In practical lithium ion battery winding equipment, \( \Psi \) is usually between 0 and 0.1. A larger taper coefficient reduces the maximum tangential stress but increases the risk of compressive tangential stress in the inner layers, which can cause wrinkles. Therefore, the selection of the tension profile must balance the maximum stress against the minimum stress.

For constant tension winding, \( F_T(r)=F_T(R)=F_{T0} \). Substituting this condition into the accumulated stress model gives the tangential stress distribution. For tapered tension winding, I substituted the tapered tension law into the same model. I then compared the stress distributions for three cylindrical lithium ion battery formats: 18650, 21700, and 46800. The material properties are listed in Table 3, and the cell specifications are listed in Table 4.

Material Density (kg/m\(^3\)) Poisson ratio Elastic limit (MPa) Thickness (mm)
Positive electrode 2700 0.35 19 0.15
Negative electrode 8960 0.32 15 0.20
Separator 897 0.392 13 0.025
Battery format Maximum winding radius (mm) Positive width (mm) Negative width (mm) Separator width (mm)
18650 9 59 60 65
21700 10.5 64 65 70
46800 23 74 75 80

I set the winding speed to 3.5 m/s and the mandrel radius to 2 mm. The negative electrode tension was adjustable from 10 N to 20 N, and the separator tension was adjustable from 5 N to 15 N. To examine the worst-case stress, I used an initial tension of 15 N. The predicted maximum tangential stress under constant tension winding is summarized in Table 5. The tangential stress first increases and then decreases as the winding radius increases. This behavior is caused by the competition between the accumulated layer pressure and the increasing outer radius. For the 46800 lithium ion battery cell, the maximum tangential stress reached 16.15 MPa, which exceeds the elastic limit of the negative electrode. Such a stress level would increase the risk of plastic deformation or fracture during high-speed winding.

Battery format Maximum tangential stress under constant tension (MPa) Elastic limit of negative electrode (MPa) Status
18650 13.42 15 Safe
21700 14.05 15 Safe
46800 16.15 15 Exceeds limit

Next, I applied tapered tension winding with \( \Psi=0.1 \). The maximum tangential stress decreased for all three formats. For the 46800 lithium ion battery cell, the maximum stress decreased by 7.8% to 14.89 MPa, which is below the elastic limit. However, the tapered tension profile also produced negative tangential stress in some inner regions. A negative tangential stress indicates compression, which can cause the separator or electrode to wrinkle. Wrinkling is particularly dangerous in a lithium ion battery because it can lead to uneven current distribution, local lithium plating, and even internal short circuits. Table 6 compares the maximum and minimum tangential stresses under constant and tapered tension.

Battery format Constant tension max stress (MPa) Tapered tension max stress (MPa) Tapered tension min stress (MPa) Observation
18650 13.42 12.51 0.82 No compression
21700 14.05 13.18 0.35 Low compression margin
46800 16.15 14.89 -0.46 Compression and wrinkling risk

The effect of the taper coefficient on the tangential stress of a 18650 lithium ion battery cell is shown in Table 7. As \( \Psi \) increases, the maximum tangential stress decreases. However, the minimum tangential stress also decreases. For a larger lithium ion battery cell, the taper coefficient must be selected carefully. If it is too large, the inner layers may enter compression and form folds. If it is too small, the maximum stress may exceed the elastic limit of the electrode or separator. For a smaller lithium ion battery cell, constant tension winding is often preferable because it is simpler to control, lower in cost, and sufficiently safe when the tension is properly selected.

Taper coefficient \( \Psi \) Maximum tangential stress (MPa) Minimum tangential stress (MPa) Risk of wrinkling
0.00 13.42 1.15 Low
0.05 13.02 0.71 Low
0.10 12.51 0.82 Low
0.15 11.96 -0.18 Moderate
0.20 11.41 -0.74 High

4. Selection of Winding Parameters for a 18650 Lithium Ion Battery

Because the winding equipment in my study was configured for a 18650 cylindrical lithium ion battery, I focused on that format for parameter selection. The negative electrode tension range was 10–20 N, and the separator tension range was 5–15 N. I evaluated the tangential stress for different working tensions. The results showed that the tangential stress remained below the elastic limit for all tested tensions, but the stress variation during winding was smallest when the negative electrode tension was near 10 N. A smaller tension variation improves layer uniformity and reduces residual stress in the final lithium ion battery cell. Therefore, I selected the following constant tension scheme: positive electrode at 10 N, negative electrode at 10 N, and separator at 5 N. The selected parameters are listed in Table 8.

Component Winding tension (N) Control mode Reason
Positive electrode 10 Constant tension Reduce stress variation and avoid plastic deformation
Negative electrode 10 Constant tension Minimize internal stress differences during winding
Separator 5 Constant tension Prevent wrinkles while maintaining stable layer contact

I also examined the sensitivity of the tangential stress to the winding speed. At a higher speed, the inertial term \( \rho V^2 \) increases, which raises the tangential stress. The effect is more pronounced in larger lithium ion battery cells because the outer radius is larger. Therefore, for high-speed winding of large-format lithium ion battery cells, the tension must be reduced or a carefully designed taper profile must be used. For the 18650 lithium ion battery cell, the selected constant tension scheme keeps the maximum tangential stress below the elastic limit even at 3.5 m/s. This combination of safety and simplicity is attractive for mass production.

5. Experimental Validation

I validated the proposed winding scheme on a high-speed lithium ion battery winding platform. The platform included active tension control for the positive electrode, negative electrode, and two separator layers. The winding speed was set to 3.5 m/s, and the mandrel radius was 2 mm. I recorded the tension values over 25 consecutive tension detection cycles. The target tension, mean tension, maximum deviation, and fluctuation range are summarized in Table 9. The tension fluctuation remained within \( \pm 5\% \), which satisfies the requirement for high-speed winding equipment. This result indicates that the constant tension controllers were able to maintain stable tension despite the increasing wound radius and the associated inertial effects.

Layer Target tension (N) Mean tension (N) Maximum deviation (N) Fluctuation range (%) Result
Positive electrode 10.0 10.03 0.21 2.10 Pass
Negative electrode 10.0 10.05 0.24 2.40 Pass
Separator 1 5.0 5.02 0.13 2.60 Pass
Separator 2 5.0 5.01 0.12 2.40 Pass

After winding, I examined the 18650 lithium ion battery cells visually and dimensionally. The wound cells were stable and uniform. I observed no bulging, no breakage, and no non-uniform winding. The outermost layer showed a small amount of separator fold, which is normal and does not affect the electrode or the electrochemical performance of the lithium ion battery. The height and diameter of six representative samples were measured. The results are listed in Table 10. The specified diameter was \( 17.0\pm0.3 \) mm, and the specified height was \( 61.0\pm0.5 \) mm. All samples were within tolerance, confirming the feasibility of the selected winding parameters.

Sample Height (mm) Diameter (mm) Height tolerance (mm) Diameter tolerance (mm) Result
1 61.24 17.20 \( 61.0\pm0.5 \) \( 17.0\pm0.3 \) Pass
2 61.25 17.18 \( 61.0\pm0.5 \) \( 17.0\pm0.3 \) Pass
3 61.22 17.18 \( 61.0\pm0.5 \) \( 17.0\pm0.3 \) Pass
4 61.28 17.20 \( 61.0\pm0.5 \) \( 17.0\pm0.3 \) Pass
5 61.18 16.90 \( 61.0\pm0.5 \) \( 17.0\pm0.3 \) Pass
6 61.21 17.12 \( 61.0\pm0.5 \) \( 17.0\pm0.3 \) Pass

The experimental results confirm that the dynamic model can guide the selection of a suitable tension control scheme for a lithium ion battery winding machine. The model captures the accumulation of tangential stress as the winding radius increases, and it explains why constant tension winding is effective for the 18650 lithium ion battery when the tension is kept at a moderate level. The model also shows that tapered tension winding can reduce the maximum stress in large-format lithium ion battery cells, but the taper coefficient must be chosen carefully to avoid compressive stress and wrinkling. These conclusions are important for the design of high-speed winding equipment and for the quality control of lithium ion battery cells.

6. Discussion

The internal stress in a wound lithium ion battery cell is a complex function of geometry, material properties, and process parameters. My model treats the wound layers as a continuum and includes the centrifugal force caused by high-speed rotation. This is a significant improvement over quasi-static models that neglect the winding speed. The centrifugal term \( \rho V^2 \) becomes increasingly important as the winding speed increases. In a high-speed lithium ion battery winding machine, the inertial force can raise the tangential stress by several percent, especially in the outer layers. If this effect is ignored, the selected tension may be too high and may cause plastic deformation.

The tangential stress distribution first increases and then decreases with the winding radius. The initial increase is caused by the accumulation of pressure from the outer layers. The later decrease occurs because the outer layers are farther from the inner core, and their constraint effect diminishes. This non-monotonic behavior means that the maximum stress does not necessarily occur at the outermost layer. Instead, it occurs at an intermediate radius. Therefore, a single tension value for all layers may not be optimal for a large lithium ion battery cell. A tapered tension profile can flatten the stress distribution and reduce the peak stress, but it can also create compression in the inner layers. The optimal taper coefficient depends on the cell format, the material properties, and the winding speed.

For the 18650 lithium ion battery, constant tension winding at 10 N for the electrodes and 5 N for the separator produced a safe stress state. The maximum tangential stress was below the elastic limit of the negative electrode, and no wrinkles or bulges were observed. The tension fluctuation was within \( \pm 5\% \), which is acceptable for high-speed production. The cell height and diameter were within tolerance. These results indicate that the constant tension scheme is practical and reliable for small cylindrical lithium ion battery cells. For larger cells, such as the 46800 format, tapered tension winding with a small taper coefficient may be necessary to keep the maximum stress below the elastic limit while avoiding compression in the inner layers.

I also note that the model assumes perfect bonding between layers and neglects friction and slip. In reality, friction between the electrode and separator can affect the stress transfer, especially when the winding speed is high. Future work could include a layer-by-layer friction model and a viscoelastic constitutive law to capture the time-dependent behavior of the separator. In addition, the thermal effect of high-speed winding could be included because the temperature rise may alter the elastic modulus and the yield strength of the lithium ion battery materials. These refinements would improve the predictive capability of the model and support the design of even higher-speed lithium ion battery winding machines.

7. Conclusions

I constructed a dynamic model for the internal stress in a cylindrical lithium ion battery cell during high-speed winding. The model is based on axisymmetric plane strain elasticity and includes the centrifugal force caused by the winding speed. The main conclusions are as follows.

1. The tangential stress in the wound lithium ion battery cell first increases and then decreases as the winding radius increases. The maximum stress occurs at an intermediate radius, not at the outer surface. The magnitude of the stress depends on the winding tension, winding speed, mandrel radius, web thickness, and material properties.

2. Tapered tension winding can reduce the maximum tangential stress compared with constant tension winding. However, if the taper coefficient is too large, the inner layers can experience compressive tangential stress, which may cause wrinkles. For the 46800 lithium ion battery cell, a taper coefficient of 0.1 reduced the maximum stress by 7.8% but produced a negative minimum stress. Therefore, the taper coefficient must be selected carefully.

3. For the 18650 lithium ion battery cell, constant tension winding is sufficient when the tension is properly selected. I chose 10 N for the positive electrode, 10 N for the negative electrode, and 5 N for the separator. The predicted maximum tangential stress remained below the elastic limit of the electrode materials.

4. Experimental validation on a high-speed winding platform showed that the tension fluctuation remained within \( \pm 5\% \). The wound lithium ion battery cells were stable, with no bulging, breakage, or non-uniform winding. The cell height and diameter were within the specified tolerances. These results confirm the feasibility of the proposed dynamic model and the selected constant tension scheme.

5. The model provides a practical basis for selecting tension control parameters in lithium ion battery winding machines. It can be extended to other cell formats and can be combined with friction, viscoelasticity, and thermal effects for further improvement. The findings are relevant to the mass production of safe and high-quality lithium ion battery cells.

Nomenclature

Symbol Definition
\( b \) Web width
\( C_1,C_2 \) Integration constants
\( E_r \) Radial elastic modulus
\( E_\theta \) Tangential elastic modulus
\( f_r \) Radial inertial force per unit volume
\( F_T \) Winding tension
\( F_{T0} \) Initial winding tension
\( p \) Contact pressure
\( r \) Radial coordinate
\( R \) Current outer radius
\( R_0 \) Mandrel radius
\( R_n \) Final outer radius
\( S \) Cross-sectional area of the web
\( T \) Web thickness
\( u \) Radial displacement
\( V \) Winding line speed
\( \varepsilon_r \) Radial strain
\( \varepsilon_\theta \) Tangential strain
\( \nu \) Poisson ratio
\( \rho \) Effective density
\( \sigma_r \) Radial stress
\( \sigma_\theta \) Tangential stress
\( \Psi \) Taper tension coefficient
\( \omega \) Angular velocity

Summary of Key Results

Item Result
Winding speed 3.5 m/s
Mandrel radius 2 mm
Selected cell format 18650 cylindrical lithium ion battery
Positive electrode tension 10 N constant
Negative electrode tension 10 N constant
Separator tension 5 N constant
Tension fluctuation Within \( \pm 5\% \)
Cell height Within \( 61.0\pm0.5 \) mm
Cell diameter Within \( 17.0\pm0.3 \) mm
Defects No bulging, breakage, or non-uniform winding

I believe that the dynamic model and the constant tension scheme presented here offer a useful engineering approach for lithium ion battery cell winding. The model can be used to predict the internal stress before production, and the experimental results can be used to verify the selected parameters. By controlling the internal stress, manufacturers can improve the quality, safety, and consistency of lithium ion battery cells. The same framework can be applied to other cylindrical lithium ion battery formats and to high-speed winding systems with different mandrel sizes and web materials.

Scroll to Top