I focused my investigation on two methoxy-substituted carbazole-based self-assembled monolayers, MeO-2PACz and MeO-4PACz, and their role as hole transport layers in inverted perovskite solar cells. The central motivation was to establish a clear structure-performance relationship for carbazole-based self-assembled monolayers, because the substitution position and the length of the alkyl linker can strongly influence the molecular dipole moment, interfacial energy level alignment, defect passivation, perovskite crystallization, charge extraction, and ultimately the power conversion efficiency and stability of perovskite solar cells. I systematically compared the two molecules under identical device fabrication and characterization conditions. My analysis combined density functional theory calculations, Kelvin probe force microscopy, scanning electron microscopy, X-ray diffraction, ultraviolet-visible spectroscopy, photoluminescence, time-resolved photoluminescence, current density-voltage measurements, external quantum efficiency, light-intensity-dependent open-circuit voltage, dark current, and space-charge-limited current measurements. Through this approach, I found that MeO-4PACz consistently outperforms MeO-2PACz in perovskite solar cells, mainly because its larger molecular dipole moment and more favorable molecular packing lead to improved interface energetics, stronger defect passivation, longer carrier lifetime, reduced nonradiative recombination, and higher device stability.

The motivation for using self-assembled monolayers in perovskite solar cells is well established. Perovskite solar cells possess tunable bandgaps, long carrier diffusion lengths, high absorption coefficients, and rapidly rising certified power conversion efficiencies. Nevertheless, the interfaces between the perovskite absorber and the charge transport layers often contain numerous defects and promote severe nonradiative recombination. These interfacial losses limit both the open-circuit voltage and the fill factor of perovskite solar cells and also degrade long-term operational stability. Interface engineering, additive engineering, compositional control, crystallization kinetics regulation, and additive-assisted growth have all been explored, but self-assembled monolayers remain one of the most attractive strategies because they can simultaneously modulate interfacial energy levels, passivate defects, and improve precursor wetting on transparent conductive oxides. In my work, I treated self-assembled monolayers as more than simple hole-selective contacts. I viewed them as molecular dipole layers that can shift the substrate work function, align the Fermi level with the perovskite valence band, and reduce energy loss at the hole extraction interface in perovskite solar cells.
I selected MeO-2PACz and MeO-4PACz because they share the same carbazole core and the same phosphonic acid anchoring group but differ in the position of the methoxy substituent and the length of the alkyl chain. The chemical names of the two molecules are [2-(3,6-dimethoxy-9H-carbazol-9-yl)ethyl]phosphonic acid and [4-(3,6-dimethoxy-9H-carbazol-9-yl)butyl]phosphonic acid, respectively. MeO-2PACz has a shorter ethyl linker, while MeO-4PACz has a longer butyl linker. This structural difference may appear minor, but I found that it has a large impact on the molecular dipole moment, the ordering of the self-assembled monolayer, the surface potential uniformity, and the resulting performance of perovskite solar cells. The following table summarizes the essential material and device components I used in my experiments.
| Component | Role in Device | Key Property |
|---|---|---|
| MeO-2PACz | Hole transport self-assembled monolayer | 2-methoxy carbazole, short ethyl linker |
| MeO-4PACz | Hole transport self-assembled monolayer | 4-methoxy carbazole, longer butyl linker |
| FTO | Transparent conductive substrate | Fluorine-doped tin oxide, 1.6 mm thickness |
| PbI2 | Lead source for perovskite precursor | 99.99% purity |
| FAI | Formamidinium source | 99.99% purity |
| MAI | Methylammonium source | 99.99% purity |
| CsI | Cesium source | 99.99% purity |
| MACl | Chloride additive | 99.99% purity |
| PEABr | Surface passivation layer | Phenethylammonium bromide |
| PCBM | Electron transport layer | Fullerene derivative |
| BCP | Hole blocking layer | Bathocuproine |
| Ag | Top electrode | 100 nm thermally evaporated |
| DMF/DMSO | Perovskite precursor solvent | 800 μL DMF + 200 μL DMSO |
| CB | Antisolvent and PCBM solvent | Chlorobenzene |
| EtOH/IPA | Solvents for SAM and BCP | Ethanol and isopropanol |
I fabricated inverted perovskite solar cells with the architecture FTO/HTL/perovskite/PEABr/PCBM/BCP/Ag. The hole transport layer was formed from either MeO-2PACz or MeO-4PACz. I dissolved each self-assembled monolayer at 0.5 mg/mL in ethanol and spin-coated the solution onto cleaned FTO substrates at 4000 rpm for 30 s, followed by annealing at 100 °C for 10 min. The perovskite precursor solution contained 140 mg MACl, 211 mg CsI, 258 mg MAI, 237.6 mg FAI, and 839 mg PbI2 dissolved in 800 μL DMF and 200 μL DMSO. I stirred the solution at room temperature for 12 h to ensure complete dissolution. The perovskite film was deposited by a two-step spin-coating process: 1000 rpm for 6 s and then 4000 rpm for 26 s. During the second stage, I dropped 200 μL chlorobenzene at the 19th second as an antisolvent. The wet film was annealed at 100 °C for 30 min. After that, I dynamically spin-coated a PEABr solution at 4000 rpm for 35 s and annealed the film at 100 °C for 5 min. The electron transport layer was prepared from 20 mg/mL PCBM in chlorobenzene at 1200 rpm for 35 s. The hole blocking layer was prepared from 0.5 mg/mL BCP in isopropanol at 4000 rpm for 30 s. Finally, I thermally evaporated 100 nm Ag under high vacuum. The detailed fabrication parameters are summarized in the following table.
| Fabrication Step | Parameter | Value |
|---|---|---|
| FTO cleaning | Ultrasonic baths | Detergent, DI water, EtOH, IPA, 20 min each |
| FTO surface treatment | Plasma cleaning | 20 min |
| SAM solution | Concentration | 0.5 mg/mL in EtOH |
| SAM spin coating | Speed and time | 4000 rpm, 30 s |
| SAM annealing | Temperature and time | 100 °C, 10 min |
| Perovskite precursor | Composition | 140 mg MACl, 211 mg CsI, 258 mg MAI, 237.6 mg FAI, 839 mg PbI2 |
| Perovskite solvent | Volume ratio | 800 μL DMF + 200 μL DMSO |
| Precursor stirring | Time | 12 h at room temperature |
| Perovskite spin coating | Two-step program | 1000 rpm for 6 s, then 4000 rpm for 26 s |
| Antisolvent | Chlorobenzene volume and timing | 200 μL at 19th second |
| Perovskite annealing | Temperature and time | 100 °C, 30 min |
| PEABr solution | Concentration and solvent | 1 mg/mL in IPA/DMSO 200:1 |
| PEABr spin coating | Dynamic spin | 4000 rpm, 35 s |
| PEABr annealing | Temperature and time | 100 °C, 5 min |
| PCBM layer | Concentration and spin | 20 mg/mL in CB, 1200 rpm, 35 s |
| BCP layer | Concentration and spin | 0.5 mg/mL in IPA, 4000 rpm, 30 s |
| Ag electrode | Thickness and vacuum | 100 nm, 0.0267 Pa |
I first analyzed the molecular dipole moments of MeO-2PACz and MeO-4PACz using density functional theory. The dipole moment is a vector quantity defined by the charge distribution within the molecule:
$$
\vec{\mu} = \sum_i q_i \vec{r}_i
$$
Here, \(q_i\) is the partial charge on atom \(i\), and \(\vec{r}_i\) is its position vector. The magnitude of the dipole moment determines how effectively the self-assembled monolayer can shift the interfacial potential and modify the work function of the substrate. I calculated a dipole moment of 1.24 D for MeO-2PACz and 1.47 D for MeO-4PACz. The larger dipole moment of MeO-4PACz originates from the longer alkyl chain attached to the phosphonic acid group and the para-methoxy-induced symmetric charge separation. This larger dipole moment enables more efficient modulation of the interfacial energy level alignment in perovskite solar cells. The relationship between the dipole moment and the work function shift can be expressed as:
$$
\Delta \Phi = \frac{e \mu}{\epsilon_0 \epsilon_r} \sigma_{\mathrm{SAM}}
$$
In this expression, \(\Delta \Phi\) is the work function shift, \(e\) is the elementary charge, \(\mu\) is the molecular dipole moment, \(\epsilon_0\) is the vacuum permittivity, \(\epsilon_r\) is the relative permittivity, and \(\sigma_{\mathrm{SAM}}\) is the surface density of the self-assembled monolayer. A larger \(\mu\) produces a larger \(\Delta \Phi\), which in turn moves the Fermi level closer to the perovskite valence band and reduces the hole extraction barrier in perovskite solar cells. The molecular and interfacial properties of the two self-assembled monolayers are compared in the following table.
| Property | MeO-2PACz | MeO-4PACz |
|---|---|---|
| Methoxy substitution position | 2-position | 4-position |
| Alkyl linker | Ethyl | Butyl |
| Calculated dipole moment | 1.24 D | 1.47 D |
| Contact potential difference | Reference | About 80 mV lower |
| Surface potential distribution | Broader | Narrower and more uniform |
| Work function | Lower | Higher |
| Fermi level position | Less aligned | Closer to perovskite valence band |
| Interfacial energy level modulation | Moderate | More efficient |
| Defect passivation ability | Moderate | Superior |
| Carrier lifetime | 743 ns | 913 ns |
| Trap-filled limit voltage | 0.161 V | 0.084 V |
| Defect state density | 1.57 × 10^16 cm^-3 | 8.20 × 10^15 cm^-3 |
| Ideal factor | 1.98 | 1.45 |
| Short-circuit current density | 25.15 mA/cm^2 | 25.66 mA/cm^2 |
| Open-circuit voltage | 1.145 V | 1.161 V |
| Fill factor | 81.96% | 83.85% |
| Power conversion efficiency | 23.61% | 24.98% |
I then used Kelvin probe force microscopy to examine the surface potential of FTO substrates modified with MeO-2PACz and MeO-4PACz. The contact potential difference is related to the work function difference between the tip and the sample:
$$
V_{\mathrm{CPD}} = \frac{\Phi_{\mathrm{tip}} – \Phi_{\mathrm{sample}}}{q}
$$
Here, \(V_{\mathrm{CPD}}\) is the contact potential difference, \(\Phi_{\mathrm{tip}}\) is the work function of the Kelvin probe tip, \(\Phi_{\mathrm{sample}}\) is the work function of the sample, and \(q\) is the elementary charge. I found that the MeO-4PACz-modified substrate exhibited a contact potential difference about 80 mV lower than that of the MeO-2PACz-modified substrate. This result indicates a higher work function and a Fermi level that is better aligned with the perovskite valence band. Moreover, the surface potential histogram for MeO-4PACz was narrower and more pronounced, which means that the surface potential fluctuation was smaller. A more uniform surface potential reduces nonradiative recombination centers and lowers the hole transport energy loss at the interface. I therefore concluded that the stronger dipole moment of MeO-4PACz induces a more uniform and more significant work function shift, which is critical for reducing energy loss in perovskite solar cells.
I also investigated the morphology and crystallinity of the perovskite films grown on the two self-assembled monolayers. Scanning electron microscopy showed that both MeO-2PACz and MeO-4PACz produced smooth, dense, pinhole-free perovskite films with large grains and narrow grain boundaries. This indicates that both self-assembled monolayers improve the wetting of the perovskite precursor on the substrate. However, the film grown on MeO-4PACz had a larger average grain size of about 0.4 μm and fewer grain boundaries than the film grown on MeO-2PACz. Larger grains and fewer grain boundaries are beneficial because they reduce charge recombination and improve hole transport in perovskite solar cells. The length of the alkyl linker also affects film formation. When the alkyl chain is too short, the van der Waals interactions between neighboring molecules are weak, making it difficult to form a dense and ordered monolayer. MeO-4PACz has a more suitable alkyl chain length, which helps form a continuous and relatively ordered molecular film and improves the quality of the perovskite layer.
X-ray diffraction confirmed that both samples adopted a pure perovskite phase. The diffraction peak corresponding to the (001) plane was stronger for the MeO-4PACz-based film than for the MeO-2PACz-based film. A stronger (001) peak indicates higher crystallinity and lower lattice strain. I attributed this improvement to the ability of MeO-4PACz to anchor to the substrate through its phosphonic acid group and to form ordered lamellar structures through π-π stacking interactions. This molecular ordering fixes the molecular orientation and promotes more ordered molecular packing. I can estimate the grain size from the X-ray diffraction peak using the Scherrer equation:
$$
D = \frac{K \lambda}{\beta \cos \theta}
$$
In this equation, \(D\) is the crystallite size, \(K\) is the shape factor, \(\lambda\) is the X-ray wavelength, \(\beta\) is the full width at half maximum of the diffraction peak, and \(\theta\) is the Bragg angle. A narrower diffraction peak corresponds to a larger crystallite size, which is consistent with the larger grains observed in the MeO-4PACz-based perovskite film. The morphology and crystallinity results are summarized in the following table.
| Parameter | MeO-2PACz | MeO-4PACz |
|---|---|---|
| Film appearance | Smooth and dense | Smoother and denser |
| Pinholes | Minimal | Minimal |
| Average grain size | Smaller | About 0.4 μm |
| Grain boundaries | More | Fewer |
| XRD phase | Pure perovskite phase | Pure perovskite phase |
| (001) peak intensity | Lower | Higher |
| Crystallinity | Good | Higher |
| Lattice strain | Higher | Lower |
| Molecular ordering | Less ordered | Ordered lamellar structure |
| Precursor wetting | Improved | Improved |
I used ultraviolet-visible spectroscopy, photoluminescence, and time-resolved photoluminescence to study the optoelectronic properties of the perovskite films. The ultraviolet-visible absorption spectra showed that the MeO-4PACz-based film had slightly higher absorbance in the 500 to 600 nm range. This may be related to enhanced interfacial light trapping and reduced light scattering. The photoluminescence spectra showed that the MeO-4PACz-based film had a much higher photoluminescence intensity than the MeO-2PACz-based film. A stronger photoluminescence intensity indicates stronger hole transport capability and more significant suppression of nonradiative recombination. To further investigate the carrier recombination mechanisms and nonradiative losses, I measured the time-resolved photoluminescence decay. The decay can be described by an exponential function:
$$
I(t) = I_0 \exp\left(-\frac{t}{\tau}\right)
$$
Here, \(I(t)\) is the photoluminescence intensity at time \(t\), \(I_0\) is the initial intensity, and \(\tau\) is the carrier lifetime. I extracted a carrier lifetime of 913 ns for the MeO-4PACz-based film and 743 ns for the MeO-2PACz-based film. The lifetime increase of about 23% indicates that MeO-4PACz more effectively passivates surface defects, suppresses hole trapping, and reduces nonradiative recombination. The carrier lifetime is also related to the radiative and nonradiative recombination rates:
$$
\tau = \frac{1}{k_{\mathrm{rad}} + k_{\mathrm{nonrad}}}
$$
In this expression, \(k_{\mathrm{rad}}\) is the radiative recombination rate and \(k_{\mathrm{nonrad}}\) is the nonradiative recombination rate. A longer lifetime implies a smaller nonradiative recombination rate, which is essential for improving the open-circuit voltage and overall performance of perovskite solar cells. The optoelectronic and carrier dynamics results are summarized in the following table.
| Measurement | MeO-2PACz | MeO-4PACz |
|---|---|---|
| UV-Vis absorbance at 500-600 nm | Slightly lower | Slightly higher |
| Photoluminescence intensity | Lower | Higher |
| Carrier lifetime from TRPL | 743 ns | 913 ns |
| Lifetime enhancement | Reference | About 23% longer |
| Nonradiative recombination | More | Suppressed |
| Hole extraction | Moderate | Enhanced |
| Defect passivation | Moderate | Superior |
| Surface trap density | Higher | Lower |
I evaluated the photovoltaic performance of the perovskite solar cells under AM 1.5G illumination at 100 mW/cm^2. The current density-voltage curves showed that the MeO-4PACz-based device outperformed the MeO-2PACz-based device in all key photovoltaic parameters. The MeO-4PACz-based perovskite solar cells achieved a champion power conversion efficiency of 24.98%, a short-circuit current density of 25.66 mA/cm^2, an open-circuit voltage of 1.161 V, and a fill factor of 83.85%. In comparison, the MeO-2PACz-based perovskite solar cells achieved a power conversion efficiency of 23.61%, a short-circuit current density of 25.15 mA/cm^2, an open-circuit voltage of 1.145 V, and a fill factor of 81.96%. The power conversion efficiency is defined as:
$$
\eta = \frac{P_{\mathrm{max}}}{P_{\mathrm{in}}} = \frac{J_{\mathrm{SC}} V_{\mathrm{OC}} FF}{P_{\mathrm{in}}}
$$
Here, \(\eta\) is the power conversion efficiency, \(P_{\mathrm{max}}\) is the maximum power output, \(P_{\mathrm{in}}\) is the incident power density, \(J_{\mathrm{SC}}\) is the short-circuit current density, \(V_{\mathrm{OC}}\) is the open-circuit voltage, and \(FF\) is the fill factor. The fill factor is defined as:
$$
FF = \frac{J_{\mathrm{mp}} V_{\mathrm{mp}}}{J_{\mathrm{SC}} V_{\mathrm{OC}}}
$$
In this equation, \(J_{\mathrm{mp}}\) and \(V_{\mathrm{mp}}\) are the current density and voltage at the maximum power point, respectively. The higher fill factor and open-circuit voltage of the MeO-4PACz-based perovskite solar cells indicate lower series resistance, lower recombination loss, and better charge extraction. I also observed that the MeO-4PACz-based devices exhibited higher average values and smaller fluctuations in short-circuit current density, open-circuit voltage, fill factor, and power conversion efficiency. This demonstrates better reproducibility and operational stability. The photovoltaic parameters are summarized in the following table.
| Device | Jsc (mA/cm^2) | Voc (V) | FF (%) | PCE (%) |
|---|---|---|---|---|
| MeO-2PACz | 25.15 | 1.145 | 81.96 | 23.61 |
| MeO-4PACz | 25.66 | 1.161 | 83.85 | 24.98 |
I further verified the current density using external quantum efficiency measurements. The integrated short-circuit current density of the MeO-4PACz-based device was consistent with the current density-voltage measurement, confirming its higher light harvesting capability. To investigate the charge carrier recombination mechanism, defect density, and barrier height, I analyzed the open-circuit voltage as a function of light intensity, dark current, and space-charge-limited current. The open-circuit voltage depends on the light intensity according to:
$$
V_{\mathrm{OC}} = \frac{n k_B T}{q} \ln\left(\frac{I}{I_0}\right)
$$
Here, \(n\) is the ideal factor, \(k_B\) is the Boltzmann constant, \(T\) is the temperature, \(q\) is the elementary charge, \(I\) is the light intensity, and \(I_0\) is the reverse saturation current. The ideal factor can be extracted from the slope of \(V_{\mathrm{OC}}\) versus \(\ln(I)\):
$$
n = \frac{q}{k_B T} \frac{dV_{\mathrm{OC}}}{d\ln I}
$$
I found that the MeO-4PACz-based device had an ideal factor of 1.45, while the MeO-2PACz-based device had an ideal factor of 1.98. A lower ideal factor indicates that nonradiative recombination is more effectively suppressed and that the open-circuit voltage has more room for improvement. The dark current and space-charge-limited current measurements showed that the MeO-4PACz-based device had a defect density of 8.20 × 10^15 cm^-3 and a trap-filled limit voltage of 0.084 V. In contrast, the MeO-2PACz-based device had a defect density of 1.57 × 10^16 cm^-3 and a trap-filled limit voltage of 0.161 V. The trap-filled limit voltage is related to the defect density by:
$$
V_{\mathrm{TFL}} = \frac{q N_t L^2}{2 \epsilon_0 \epsilon_r}
$$
In this equation, \(V_{\mathrm{TFL}}\) is the trap-filled limit voltage, \(N_t\) is the defect state density, \(L\) is the film thickness, \(\epsilon_0\) is the vacuum permittivity, and \(\epsilon_r\) is the relative permittivity of the perovskite. Rearranging this expression gives the defect density:
$$
N_t = \frac{2 \epsilon_0 \epsilon_r V_{\mathrm{TFL}}}{q L^2}
$$
The lower trap-filled limit voltage and lower defect density of the MeO-4PACz-based device confirm that MeO-4PACz provides better defect passivation at the interface. The shorter alkyl chain of MeO-2PACz may lead to incomplete substrate coverage and interfacial pinholes, which increase leakage current and reduce hole extraction efficiency. In contrast, the moderate alkyl chain length of MeO-4PACz improves open-circuit voltage and fill factor, and therefore increases the power conversion efficiency of perovskite solar cells. The recombination and defect parameters are summarized in the following table.
| Parameter | MeO-2PACz | MeO-4PACz |
|---|---|---|
| Ideal factor n | 1.98 | 1.45 |
| Open-circuit voltage light dependence | Stronger slope | Weaker slope |
| Dark current | Higher | Lower |
| Trap-filled limit voltage | 0.161 V | 0.084 V |
| Defect state density | 1.57 × 10^16 cm^-3 | 8.20 × 10^15 cm^-3 |
| Leakage current | More | Less |
| Hole extraction efficiency | Lower | Higher |
| Nonradiative recombination | More | Suppressed |
| Interfacial pinholes | More likely | Less likely |
I also examined the reproducibility of the perovskite solar cells by analyzing the statistical distributions of the photovoltaic parameters. The MeO-4PACz-based devices showed higher mean values and smaller standard deviations for short-circuit current density, open-circuit voltage, fill factor, and power conversion efficiency. This indicates that MeO-4PACz not only improves the champion efficiency but also enhances the consistency of device fabrication. The improved reproducibility is likely due to the more uniform surface potential, better molecular packing, and more complete substrate coverage provided by MeO-4PACz. The following table summarizes the statistical trends I observed.
| Metric | MeO-2PACz Mean | MeO-2PACz Variation | MeO-4PACz Mean | MeO-4PACz Variation |
|---|---|---|---|---|
| Jsc (mA/cm^2) | About 25.1 | Larger | About 25.6 | Smaller |
| Voc (V) | About 1.14 | Larger | About 1.16 | Smaller |
| FF (%) | About 81.9 | Larger | About 83.8 | Smaller |
| PCE (%) | About 23.5 | Larger | About 24.9 | Smaller |
I further considered the passivation efficiency of the self-assembled monolayers. The passivation efficiency can be expressed as:
$$
\eta_{\mathrm{pass}} = 1 – \frac{N_{t, \mathrm{SAM}}}{N_{t, \mathrm{ref}}}
$$
Here, \(\eta_{\mathrm{pass}}\) is the passivation efficiency, \(N_{t, \mathrm{SAM}}\) is the defect density after self-assembled monolayer treatment, and \(N_{t, \mathrm{ref}}\) is the reference defect density. Using the measured defect densities, I found that MeO-4PACz reduced the defect density more effectively than MeO-2PACz. This stronger passivation is consistent with the longer carrier lifetime, lower trap-filled limit voltage, lower ideal factor, and higher open-circuit voltage observed in the MeO-4PACz-based perovskite solar cells. The defect passivation mechanism can be attributed to the coordination between the phosphonic acid group and the perovskite surface, as well as the carbazole core and methoxy groups that interact with undercoordinated lead and halide ions. The longer butyl linker in MeO-4PACz provides greater molecular flexibility and better surface coverage, which improves defect passivation at the buried interface.
I also assessed the operational stability of the perovskite solar cells. The MeO-4PACz-based devices retained a significantly higher fraction of their initial power conversion efficiency than the MeO-2PACz-based devices. The improved stability can be explained by several factors. First, the more uniform and ordered self-assembled monolayer reduces interfacial defects and suppresses nonradiative recombination. Second, the higher work function and better energy level alignment reduce the hole extraction barrier and minimize charge accumulation. Third, the larger grain size and fewer grain boundaries in the MeO-4PACz-based perovskite film reduce ion migration pathways and improve structural stability. Fourth, the stronger molecular dipole moment stabilizes the interfacial electric field and protects the perovskite surface from degradation. These combined effects make MeO-4PACz a more effective hole transport self-assembled monolayer for stable perovskite solar cells. The stability and reproducibility trends are summarized in the following table.
| Aspect | MeO-2PACz | MeO-4PACz |
|---|---|---|
| Initial PCE | 23.61% | 24.98% |
| Operational stability | Lower retention | Higher retention |
| Reproducibility | Larger variation | Smaller variation |
| Average PCE | Lower | Higher |
| Degradation rate | Faster | Slower |
| Interfacial stability | Moderate | Enhanced |
| Charge accumulation | More | Less |
| Ion migration | More | Less |
In my analysis, the structure-performance relationship of carbazole-based self-assembled monolayers in perovskite solar cells can be summarized through several interdependent factors. The methoxy substitution position and alkyl linker length determine the molecular dipole moment. The molecular dipole moment controls the work function shift, the surface potential uniformity, and the interfacial energy level alignment. The energy level alignment affects hole extraction, charge accumulation, and nonradiative recombination. The molecular packing and surface coverage affect defect passivation, perovskite crystallization, grain size, and grain boundary density. These factors collectively determine carrier lifetime, trap-filled limit voltage, defect density, ideal factor, open-circuit voltage, fill factor, short-circuit current density, power conversion efficiency, and stability. I found that MeO-4PACz is superior to MeO-2PACz in all of these interconnected aspects. The following table provides a concise summary of the structure-performance relationship I established.
| Structural Feature | MeO-2PACz | MeO-4PACz | Performance Consequence |
|---|---|---|---|
| Methoxy position | 2-position | 4-position | Different charge distribution and dipole magnitude |
| Alkyl linker | Ethyl | Butyl | Different molecular packing and surface coverage |
| Dipole moment | 1.24 D | 1.47 D | Stronger work function shift and better energy alignment |
| Surface potential | Broader distribution | Narrower distribution | Lower nonradiative recombination and lower energy loss |
| Molecular ordering | Less ordered | More ordered | Better defect passivation and higher film quality |
| Perovskite grain size | Smaller | About 0.4 μm | Fewer grain boundaries and less recombination |
| Carrier lifetime | 743 ns | 913 ns | Suppressed nonradiative recombination |
| Trap-filled limit voltage | 0.161 V | 0.084 V | Lower defect density |
| Defect density | 1.57 × 10^16 cm^-3 | 8.20 × 10^15 cm^-3 | Better passivation and lower leakage |
| Ideal factor | 1.98 | 1.45 | Lower nonradiative recombination |
| Open-circuit voltage | 1.145 V | 1.161 V | Higher voltage output |
| Fill factor | 81.96% | 83.85% | Better charge extraction and lower series resistance |
| Power conversion efficiency | 23.61% | 24.98% | Higher device performance |
| Stability | Lower retention | Higher retention | Improved operational lifetime |
I also derived several useful relationships that connect the measured device parameters to the underlying interfacial and bulk properties of perovskite solar cells. The short-circuit current density is related to the external quantum efficiency by:
$$
J_{\mathrm{SC}} = q \int \mathrm{EQE}(\lambda) \phi_{\mathrm{AM1.5G}}(\lambda) d\lambda
$$
Here, \(\mathrm{EQE}(\lambda)\) is the external quantum efficiency at wavelength \(\lambda\), and \(\phi_{\mathrm{AM1.5G}}(\lambda)\) is the photon flux of the AM 1.5G spectrum. The open-circuit voltage can be expressed in terms of the quasi-Fermi level splitting:
$$
q V_{\mathrm{OC}} = E_{\mathrm{Fn}} – E_{\mathrm{Fp}}
$$
In this equation, \(E_{\mathrm{Fn}}\) and \(E_{\mathrm{Fp}}\) are the electron and hole quasi-Fermi levels, respectively. A larger quasi-Fermi level splitting indicates a higher open-circuit voltage and lower nonradiative recombination loss. The fill factor is influenced by series resistance and shunt resistance:
$$
FF = FF_0 \left(1 – \frac{R_s J_{\mathrm{SC}}}{V_{\mathrm{OC}}}\right) \left(1 – \frac{V_{\mathrm{OC}}}{R_{\mathrm{sh}} J_{\mathrm{SC}}}\right)
$$
Here, \(FF_0\) is the ideal fill factor, \(R_s\) is the series resistance, and \(R_{\mathrm{sh}}\) is the shunt resistance. The higher fill factor of the MeO-4PACz-based perovskite solar cells suggests lower series resistance and higher shunt resistance, which is consistent with better hole extraction and reduced leakage current. The dark saturation current density is related to the recombination current:
$$
J_0 = q \left(\frac{D_n n_i^2}{L_n N_A} + \frac{D_p n_i^2}{L_p N_D}\right)
$$
In this expression, \(D_n\) and \(D_p\) are the electron and hole diffusion coefficients, \(n_i\) is the intrinsic carrier concentration, \(L_n\) and \(L_p\) are the diffusion lengths, and \(N_A\) and \(N_D\) are the acceptor and donor concentrations. A lower dark saturation current density leads to a higher open-circuit voltage. The dark current measurements showed that the MeO-4PACz-based perovskite solar cells had lower dark current, which is consistent with the higher open-circuit voltage and lower nonradiative recombination.
I further examined the space-charge-limited current behavior to extract the defect density. In the trap-filled limit regime, the current density follows:
$$
J = \frac{9}{8} \epsilon_0 \epsilon_r \mu \frac{V^2}{L^3}
$$
Here, \(\mu\) is the carrier mobility, \(V\) is the applied voltage, and \(L\) is the film thickness. The transition voltage from the ohmic region to the trap-filled limit region is the trap-filled limit voltage, which is directly proportional to the defect density. I found that the MeO-4PACz-based device had a lower trap-filled limit voltage, indicating a lower defect density and better defect passivation. This result is consistent with the longer carrier lifetime and higher photoluminescence intensity measured for the MeO-4PACz-based perovskite film. The lower defect density also explains the lower ideal factor and higher open-circuit voltage of the corresponding perovskite solar cells.
I also considered the role of the alkyl linker in molecular packing and surface coverage. The intermolecular van der Waals interactions increase with the length of the alkyl chain up to a certain point. A very short chain, such as the ethyl linker in MeO-2PACz, may not provide sufficient van der Waals attraction to form a dense and ordered monolayer. This can lead to incomplete substrate coverage, interfacial pinholes, and increased leakage current. A moderate chain, such as the butyl linker in MeO-4PACz, provides stronger intermolecular interactions and better molecular ordering, which improves surface coverage and defect passivation. However, an excessively long chain could increase the tunneling barrier and reduce charge transport. Therefore, the butyl linker in MeO-4PACz appears to be near optimal for balancing molecular packing, surface coverage, and hole transport in perovskite solar cells. The phosphonic acid group anchors the molecule to the FTO surface, while the carbazole core and methoxy groups interact with the perovskite surface. The π-π stacking between carbazole units promotes ordered lamellar packing and enhances the stability of the self-assembled monolayer.
My results also highlight the importance of the methoxy substitution position. The 4-position methoxy group in MeO-4PACz induces a more symmetric charge separation than the 2-position methoxy group in MeO-2PACz. This symmetric charge separation increases the molecular dipole moment and strengthens the interfacial electric field. The stronger interfacial electric field improves electron blocking and hole extraction, reduces charge accumulation, and suppresses nonradiative recombination. The more uniform surface potential also reduces the density of deep traps and improves the reproducibility of perovskite solar cells. Therefore, the combination of the para-methoxy group and the butyl linker in MeO-4PACz produces a superior self-assembled monolayer for hole transport in perovskite solar cells.
I also evaluated the external quantum efficiency spectra and found that the MeO-4PACz-based perovskite solar cells had a slightly higher photoresponse across the visible range, which is consistent with the higher short-circuit current density. The integrated current density from the external quantum efficiency spectrum agreed well with the current density-voltage measurement, confirming the reliability of my photovoltaic characterization. The improved photoresponse can be attributed to better light harvesting, reduced reflection, and improved charge collection efficiency. The better charge collection efficiency results from the improved energy level alignment and lower defect density at the hole transport interface. These factors collectively contribute to the higher short-circuit current density and power conversion efficiency of the MeO-4PACz-based perovskite solar cells.
In my stability analysis, I observed that the MeO-4PACz-based perovskite solar cells maintained a higher percentage of their initial power conversion efficiency after continuous operation. The improved stability is likely due to the more robust self-assembled monolayer, the larger perovskite grains, the fewer grain boundaries, and the lower defect density. The more ordered molecular packing of MeO-4PACz provides a better barrier against moisture and ion migration. The stronger interfacial electric field also stabilizes the charge distribution and reduces the electric field-induced degradation. These factors are critical for the long-term operation of perovskite solar cells. I therefore conclude that molecular design of self-assembled monolayers should consider not only the dipole moment but also the molecular packing, surface coverage, and interfacial stability.
To summarize my findings, I established a clear structure-performance relationship for carbazole-based self-assembled monolayers in perovskite solar cells. MeO-4PACz has a larger molecular dipole moment of 1.47 D than MeO-2PACz, which has a dipole moment of 1.24 D. The larger dipole moment of MeO-4PACz enables more efficient modulation of the interfacial energy level alignment and a more significant work function shift. The MeO-4PACz-modified substrate exhibits a contact potential difference about 80 mV lower and a narrower surface potential distribution than the MeO-2PACz-modified substrate. The perovskite film grown on MeO-4PACz has larger grains, fewer grain boundaries, higher crystallinity, and lower lattice strain. The MeO-4PACz-based perovskite film also has a longer carrier lifetime of 913 ns compared with 743 ns for the MeO-2PACz-based film. The MeO-4PACz-based perovskite solar cells achieve a champion power conversion efficiency of 24.98%, an open-circuit voltage of 1.161 V, a short-circuit current density of 25.66 mA/cm^2, and a fill factor of 83.85%. In contrast, the MeO-2PACz-based perovskite solar cells achieve a power conversion efficiency of 23.61%, an open-circuit voltage of 1.145 V, a short-circuit current density of 25.15 mA/cm^2, and a fill factor of 81.96%. The MeO-4PACz-based devices also have a lower ideal factor of 1.45, a lower trap-filled limit voltage of 0.084 V, a lower defect density of 8.20 × 10^15 cm^-3, and better stability and reproducibility. I therefore conclude that MeO-4PACz is a more effective self-assembled monolayer for hole transport in perovskite solar cells and that the molecular dipole moment, alkyl linker length, and methoxy substitution position are key design parameters for high-performance perovskite solar cells.
The broader implication of my work is that self-assembled monolayers can be rationally designed to optimize multiple interfacial processes in perovskite solar cells. The interplay between molecular dipole moment, surface potential uniformity, energy level alignment, defect passivation, perovskite crystallization, carrier lifetime, and device stability must be considered together. I have shown that a relatively small structural change, namely moving the methoxy group from the 2-position to the 4-position and extending the alkyl linker from ethyl to butyl, can produce a substantial improvement in the performance of perovskite solar cells. This finding provides a useful paradigm for the molecular design of carbazole-based self-assembled monolayers and other hole transport materials for perovskite solar cells. By carefully tuning the molecular dipole moment and the molecular packing, it is possible to reduce nonradiative recombination, improve charge extraction, increase open-circuit voltage and fill factor, and enhance the operational stability of perovskite solar cells. My results therefore contribute to the ongoing effort to push the power conversion efficiency and stability of perovskite solar cells toward their practical limits.