The pursuit of high energy density and long cycle life has established the lithium-ion battery as the cornerstone of modern portable electronics and electric vehicles. However, the inherent safety risks, particularly thermal runaway leading to fire or explosion, remain a significant concern. A primary precursor to such catastrophic failure is an internal short circuit (ISC), often initiated by electrical abuse like overcharging or overdischarge. In battery packs, cell-to-cell capacity variations can lead to smaller-capacity cells being driven into overdischarge during operation. While conventional Battery Management Systems (BMS) monitor parameters like voltage and temperature, these signals offer limited sensitivity for detecting the nascent stage of an ISC, especially one induced by overdischarge, which evolves gradually with subtle initial electrical and thermal signatures. Therefore, developing a reliable, online diagnostic method for early-stage ISC detection is paramount for enhancing the safety of li ion battery systems.

Electrochemical Impedance Spectroscopy (EIS) is a powerful non-invasive technique that probes the internal state of a li ion battery by analyzing its response to a small-signal AC perturbation. The impedance spectrum reveals information about various internal processes, including charge transfer, solid-electrolyte interphase (SEI) layer properties, and ion diffusion. Consequently, impedance is a highly sensitive indicator of internal degradation and fault conditions. This article investigates the mechanistic link between overdischarge and ISC formation, develops a tailored online impedance measurement device, and proposes a novel, model-free diagnostic method based on dynamic impedance characteristics at a specific frequency to reliably identify and provide early warning for overdischarge-induced ISC in li ion battery cells.
Mechanism of Overdischarge-Induced Internal Short Circuit
During normal discharge of a li ion battery, lithium ions de-intercalate from the anode and intercalate into the cathode. As the terminal voltage approaches the cut-off limit, the de-intercalation process nears completion. Forcing the cell beyond this point—overdischarge—triggers a cascade of deleterious side reactions. The process can be segmented into three distinct stages based on terminal voltage behavior, as illustrated conceptually below.
Stage I (Rapid Voltage Drop): Post cut-off voltage, excessive lithium removal raises the anode potential, causing a sharp decline in cell voltage. The low potential destabilizes the SEI layer, leading to its partial decomposition. While this stage is partially reversible if halted promptly, it marks the onset of degradation.
Stage II (Voltage Recovery & Copper Dissolution): This is the critical phase for ISC initiation. As the anode potential rises further to the corrosion potential of the copper current collector, oxidation occurs:
$$ \text{Cu} \rightarrow \text{Cu}^{2+} + 2e^- $$
The dissolved copper ions ($\text{Cu}^{2+}$) migrate through the electrolyte towards the cathode. Upon reaching the cathode, they are reduced and deposit as metallic copper:
$$ \text{Cu}^{2+} + 2e^- \rightarrow \text{Cu} $$
This deposition forms a copper layer on the cathode surface and, more critically, dendritic copper structures that can grow through the separator. The deposition of copper on the cathode increases its potential, manifesting as a recovery in the measured cell voltage. The growth of copper dendrites is the primary mechanical driver for an ISC, as they can eventually pierce the separator and create an electronic bridge between the anode and cathode.
Stage III (Voltage Plateau and ISC Evolution): The dissolution and deposition reactions continue. As dendrites grow and make contact, a micro-short circuit is established. The severity of this ISC increases with overdischarge depth, lowering the internal short resistance and potentially leading to thermal runaway.
The impedance of a li ion battery is commonly represented by an equivalent circuit model (ECM). A typical model includes elements for ohmic resistance ($R_\Omega$), SEI layer impedance ($R_{SEI}$), charge transfer resistance ($R_{ct}$), and a Warburg element ($W$) for diffusion. Overdischarge impacts each element:
- $R_\Omega$: Increases due to electrolyte decomposition reducing ionic conductivity.
- $R_{SEI}$: Decreases due to the decomposition of the SEI layer.
- $R_{ct}$: Increases significantly due to structural damage at the anode (graphite detachment from the dissolved copper current collector) hindering charge transfer kinetics.
- Warburg Impedance: Increases as the diffusion of ions is hampered by the degraded electrode structure and side reaction products.
Therefore, monitoring the dynamic evolution of impedance, particularly components like $R_{ct}$, provides a direct window into the internal degradation processes that culminate in an ISC.
Design of an Online Impedance Measurement Device
To enable real-time, in-situ impedance monitoring during battery operation, a dedicated measurement device was designed and built. The core requirement was to inject a small, non-disruptive AC current signal into the li ion battery and precisely measure the voltage response across it and a reference shunt resistor. The device was based on an embedded microcontroller and employed a four-wire (Kelvin) measurement technique to eliminate lead resistance errors.
The system architecture comprises several key modules:
- Signal Generation: A Direct Digital Synthesizer (DDS) generates a pure, digitally programmable sine wave voltage at the target frequency (e.g., 70 Hz). This signal is amplified and converted into a current signal using a voltage-to-current converter. The excitation current amplitude is set to a low value (e.g., C/20) to ensure linearity and non-invasiveness.
- Signal Acquisition: The voltage responses across a precision shunt resistor ($R_{shunt}$) and the li ion battery under test are measured simultaneously via a dual-channel, synchronous Analog-to-Digital Converter (ADC). High-resolution ADCs (e.g., 16-bit or 24-bit) are used to capture the small AC signals superimposed on the large DC bias of the operating battery.
- Signal Processing & Impedance Calculation: To accurately extract the amplitude and phase of the AC components from the sampled time-domain data, an all-phase Fast Fourier Transform (apFFT) algorithm was implemented. Compared to standard FFT, apFFT offers superior phase estimation and reduced spectral leakage, which is crucial for precise impedance calculation, especially with limited data windows suitable for online use. The impedance magnitude $|Z|$ and phase $\phi$ at the excitation frequency $\omega$ are calculated as follows:
$$ |Z(\omega)| = \frac{U_{bat}(\omega)}{I(\omega)} = \frac{U_{bat}(\omega)}{U_{shunt}(\omega)} \times R_{shunt} $$
$$ \phi(\omega) = \phi_{U_{bat}}(\omega) – \phi_{U_{shunt}}(\omega) $$
where $U_{bat}$ and $U_{shunt}$ are the complex AC voltage amplitudes across the battery and shunt, respectively. The real and imaginary parts are then:
$$ Z_{real} = |Z| \cdot \cos(\phi) $$
$$ Z_{imag} = |Z| \cdot \sin(\phi) $$
This device can operate in two modes: a sweep mode to obtain full EIS spectra during static conditions, and a fixed-frequency mode for continuous, high-speed dynamic impedance monitoring during charge/discharge cycles, which is essential for fault diagnosis.
Selection of Characteristic Monitoring Frequency
A critical step for reliable online diagnosis is to select an impedance measurement frequency that is primarily sensitive to the fault mechanism (ISC development) while being relatively decoupled from normal operational state variations, chiefly State of Charge (SOC) and temperature. Extensive EIS measurements were conducted on li ion battery cells across a range of SOCs (10% to 90%) and temperatures (5°C to 45°C). Analysis of the resulting Nyquist plots revealed distinct frequency-dependent behaviors:
| Frequency Band | Dominant Process | Dependence on SOC & Temperature |
|---|---|---|
| Very High (1-10 kHz) | Ohmic resistance, inductance | Low SOC dependence, minor temperature effect. |
| High (40-1000 Hz) | SEI layer, start of charge transfer | Low SOC dependence in lower part (40-100 Hz). Temperature effect present. |
| Mid (1-40 Hz) | Charge transfer kinetics | Strong SOC and temperature dependence. |
| Low (0.01-1 Hz) | Lithium-ion diffusion | Strong SOC (at extremes) and temperature dependence. |
The impedance in the **40 Hz to 100 Hz** range showed the most consistent behavior across different SOC levels, minimizing false alarms due to normal SOC changes during discharge. Furthermore, a higher frequency allows for faster measurement, which is crucial for real-time monitoring. Therefore, **70 Hz** was selected as the characteristic monitoring frequency. At this frequency, the impedance is influenced by both the SEI layer and the charge transfer process, making it a sensitive probe for the degradation of these interfaces during overdischarge, while providing a stable baseline during normal operation.
Impedance Response During Normal and Overdischarge Operation
Experiments were conducted on commercial 18650 LiFePO4/Graphite cells. First, the dynamic impedance at 70 Hz was recorded during standard 1C charge and discharge cycles to establish a baseline. Subsequently, overdischarge tests were performed by assembling a pack where one cell (initial SOC=50%) was forced into overdischarge by 20% SOC relative to its full capacity, while other cells in the pack provided the load path. The target cell’s voltage, surface temperature, and dynamic impedance were monitored simultaneously.
1. Normal Discharge and Charge
During a standard constant-current (CC) discharge, the 70 Hz impedance showed a slight, gradual decrease. This is attributed to the competing effects of increasing temperature (which lowers $R_{ct}$) and decreasing SOC (which tends to increase $R_{ct}$). A distinct and highly reproducible feature was observed near the end of discharge: a rapid, transient “semi-sinusoidal” spike in impedance just before the voltage cut-off. This is caused by severe concentration polarization as lithium-ion depletion occurs at the electrodes.
During charging, the impedance trend was more stable, with a small drop during the CC phase and a gradual rise during the constant-voltage (CV) phase.
2. Overdischarge to Failure
The overdischarge process revealed critical impedance signatures that correlate with the degradation stages. The key results are summarized in the table below, comparing the warning time provided by different parameters.
| Diagnostic Parameter | Key Observed Feature | Event Signified | Lead Time Before ISC | Limitation/Advantage |
|---|---|---|---|---|
| Terminal Voltage | Rapid drop near cut-off | Approaching overdischarge | ~13 s before overdischarge starts | Very short warning; no clear ISC signature. |
| Surface Temperature | Rapid rise | Onset of exothermic side reactions | ~45 s after overdischarge starts | Lagging indicator; mild temperature rise (<32°C). |
| Dynamic Impedance @ 70 Hz | 1. Semi-sinusoidal spike 2. Needle-like spike 3. Significant sustained rise |
1. End of normal discharge (Overdischarge Warning) 2. Pre-ISC structural damage (ISC Warning) 3. ISC Formation |
1. ~144 s before overdischarge 2. ~152 s before ISC 3. 0 s (ISC occurrence marker) |
Provides multi-stage, early warning with clear features. |
| Impedance Change Rate (d|Z|/dt) | 1. Pseudo-sinusoidal peak 2. Sharper pseudo-sinusoidal peak 3. Small凸起 (bump) |
Same events as above | 1. ~3 s earlier than Feature 1 2. ~5 s earlier than Feature 2 3. ~2 s earlier than Feature 3 |
Amplifies rate of change, enabling even earlier algorithm triggering. |
The sequence of impedance features provides a clear diagnostic roadmap:
Feature 1 (Semi-sinusoidal Spike): This is identical to the normal end-of-discharge polarization spike. Its detection serves as an overdischarge warning, signaling that the cell is about to be driven below its safe operating voltage. Detecting this provides ample time (~144 s) for the BMS to intervene (e.g., initiate balancing or disconnect the load).
Feature 2 (Needle-like Spike): After the cell enters overdischarge, a second, sharper impedance spike appears. This corresponds to the onset of SEI decomposition and initial structural damage to the anode, preceding copper dissolution. This is the critical ISC warning.
Feature 3 (Sustained Impedance Rise): Following the warning spike, the impedance drops slightly and then begins a pronounced, monotonic increase. This marks the period of active copper dissolution, dendrite growth, and the eventual formation of a stable internal short circuit. This feature is a clear confirmation of ISC occurrence.
The derivative of the impedance (rate of change) provides an even more sensitive indicator, with distinctive peaks corresponding to each of the three main features, offering a few seconds of additional lead time for algorithm-based detection.
Experimental Validation of the Diagnostic Method
The diagnostic capability of the dynamic impedance features was rigorously validated through post-test capacity analysis and cell teardown. Four identical li ion battery cells were subjected to different discharge termination points based on the impedance features:
- Cell Ref: Discharged to standard cut-off voltage (2.0V).
- Cell Warn_OD: Discharge terminated at the first impedance spike (Overdischarge Warning).
- Cell Warn_ISC: Discharge terminated at the second impedance spike (ISC Warning).
- Cell ISC: Discharge terminated after the sustained impedance rise began (ISC Confirmed).
All cells were then fully recharged and subjected to capacity check tests and a long-term open-circuit stand to measure self-discharge. The results are summarized below:
| Cell ID | Termination Point | Irreversible Capacity Loss | Self-Discharge Rate | Post-Test Teardown Observation |
|---|---|---|---|---|
| Ref | Cut-off Voltage | Negligible (< 0.3%) | Normal | Intact electrodes and separator. |
| Warn_OD | Feature 1 (Semi-sinusoidal Spike) | Negligible (< 0.3%) | Normal | No visible damage. Functionally identical to Ref cell. |
| Warn_ISC | Feature 2 (Needle-like Spike) | Small Increase (~2%) | Slightly Elevated | Minor anode surface changes. Accelerated aging in subsequent cycles but remains functional. |
| ISC | Feature 3 (Sustained Rise) | Large (> 4%) | Severely Elevated (>10% in 72h) | Clear evidence of ISC: Yellow copper deposition on cathode, damaged graphite anode, dissolved copper current collector, and pierced/contaminated separator. |
The validation confirms the proposed method’s accuracy:
- Feature 1 is a safe warning threshold. Halting discharge here prevents any measurable damage to the li ion battery.
- Feature 2 is a critical warning threshold. While it causes some irreversible capacity loss, stopping here prevents the catastrophic copper dissolution process, preserving most of the cell’s functionality and preventing a hard ISC.
- Feature 3 is a failure confirmation marker. Cells stopped here already have an established ISC, exhibiting high self-discharge and clear physical damage, confirming the fault.
Conclusion
This study successfully demonstrates a novel, model-free online diagnostic method for identifying overdischarge-induced internal short circuits in li ion battery cells. By analyzing the mechanistic link between overdischarge, copper dissolution, and impedance change, a characteristic monitoring frequency of 70 Hz was identified. Using a purpose-built online impedance measurement device, three distinct dynamic impedance features were extracted during the overdischarge process:
- The semi-sinusoidal spike provides an early overdischarge warning ~144 seconds before the cell is forced beyond its cut-off voltage.
- The needle-like spike serves as an internal short circuit warning ~152 seconds before the ISC fully forms, corresponding to the onset of severe structural damage.
- The sustained impedance rise acts as a definitive marker for ISC occurrence.
Furthermore, monitoring the impedance change rate can provide even earlier detection triggers. This method overcomes the limitations of conventional voltage and temperature monitoring, which offer short or lagging warnings with poor specificity for early-stage ISCs. The proposed technique, requiring only single-frequency impedance measurement and simple feature detection algorithms, is computationally efficient and highly suitable for integration into existing BMS platforms, offering a significant advancement towards safer and more reliable li ion battery systems.