I have focused my recent work on the metallization of perovskite solar cells because these devices offer one of the most promising routes toward ultra-high photovoltaic conversion efficiency. In my view, the conductive paste is not merely an auxiliary material; it is a critical enabler for the commercialization of perovskite solar cells. The reason is straightforward: perovskite solar cells require a low-temperature metallization process, typically not exceeding 150 °C, whereas conventional crystalline silicon solar cells often tolerate firing temperatures above 700 °C. This thermal constraint changes the entire design philosophy of the conductive powder, the organic vehicle, and the curing chemistry. In the following sections, I describe my systematic investigation of silver powder and silver-coated copper powder for perovskite solar cells, with a focus on volume resistivity, contact resistivity, curing behavior, and cost reduction.

Perovskite solar cells are third-generation photovoltaic devices with a general material formula of ABX3, where A is typically an organic cation, B is a metal cation, and X is a halide anion. I have noted that single-junction perovskite solar cells have a theoretical conversion efficiency of approximately 33%, while perovskite tandem solar cells, especially perovskite/silicon two-junction tandems, can exceed 40% theoretical efficiency. These values explain why perovskite solar cells have attracted intense research and industrial interest. However, the commercialization of perovskite solar cells still faces challenges such as large-area module efficiency loss, long-term stability, and pronounced efficiency degradation. One of the most practical bottlenecks is the metallization step. Because many perovskite compositions, such as CsPbBr3, require low annealing temperatures around 150 °C to achieve high coverage and high crystallinity, any high-temperature process can destroy the perovskite structure. Therefore, the conductive paste used in perovskite solar cells must cure below 150 °C. This requirement is even stricter than that for heterojunction solar cells, and it places high demands on the conductive powders, organic carriers, and curing agents.
In my experimental work, I adopted a production-compatible curing schedule for perovskite solar cells: drying at 90 °C for 3 minutes to remove organic solvents, followed by curing at 150 °C for 10 minutes to complete metallization. This schedule allows the conductive powders to form stable conductive pathways and to achieve good electrical contact with the perovskite cell. To reduce cost, I also explored silver-coated copper powder as a partial replacement for silver powder. With a well-designed silver-coated copper powder, the silver content in the conductive paste can be reduced to 30% or even below, which significantly lowers the cost per kilogram of paste. The central question I address is how the particle size and type of conductive powder affect the electrical performance of perovskite solar cells.
I selected a bisphenol F epoxy resin as the main resin because of its low molecular weight and high reactivity. I used 2-ethyl-4-methylimidazole as the curing agent, which can react rapidly with bisphenol F epoxy at 120 °C. This combination provides a latent curing system that is stable at room temperature and has a long pot life. For the solvent system, I chose N-methylpyrrolidone and diethylene glycol butyl ether acetate. These two solvents have different volatilities, creating a temperature-gradient evaporation profile. This gradient helps maintain screen-printing performance while still allowing good low-temperature volatility. In perovskite solar cells, the conductive powder accounts for more than 90% of the paste mass, so optimizing the powder blend is essential for maximizing packing density, interparticle contact, and electrical performance.
The conductive powders I studied included spherical silver powders with average particle sizes (D50) of 0.35 μm, 0.55 μm, 1.02 μm, 1.55 μm, and 2.01 μm. All silver powders were treated with the same surface coating agent to ensure good dispersion. I also studied spherical silver-coated copper powders with a silver content of 20% and average particle sizes of 0.41 μm, 0.61 μm, 1.15 μm, 1.62 μm, and 2.08 μm. These powders were also treated with a uniform surface coating agent. Using these materials, I prepared conductive pastes for perovskite solar cells and compared the volume resistivity and contact resistivity of the screen-printed grid electrodes after curing at 90 °C for 3 minutes and 150 °C for 10 minutes.
The fundamental electrical relationships I used to evaluate the metallization of perovskite solar cells are as follows. The volume resistivity of a grid line is given by:
$$\rho = R \frac{A}{L}$$
where \(R\) is the measured resistance, \(A\) is the cross-sectional area, and \(L\) is the length of the conductor. For a four-point probe measurement on a thin film or printed line, the sheet resistance can be expressed as:
$$R_s = \frac{\rho}{t}$$
where \(t\) is the thickness. In my four-point probe measurements, I used the standard correction:
$$\rho = \frac{\pi}{\ln 2} t \frac{V}{I} f$$
where \(V\) is the measured voltage, \(I\) is the injected current, and \(f\) is a geometry correction factor. The contact resistivity between the grid line and the underlying silicon or perovskite interface is defined as:
$$\rho_c = R_c A_c$$
where \(R_c\) is the contact resistance and \(A_c\) is the contact area. For a composite conductive paste, the percolation behavior can be described by:
$$\sigma = \sigma_0 (\phi – \phi_c)^t$$
where \(\sigma\) is the composite conductivity, \(\sigma_0\) is a scaling constant, \(\phi\) is the conductive filler volume fraction, \(\phi_c\) is the percolation threshold, and \(t\) is the critical exponent. In my pastes, the volume fraction of conductive powder is very high, typically above 50 vol%, so the system is well above the percolation threshold. However, the number of interparticle contacts and the contact area still dominate the final resistivity. I also considered the effective medium approximation:
$$\frac{\sigma – \sigma_m}{\sigma + 2\sigma_m} = \phi \frac{\sigma_p – \sigma_m}{\sigma_p + 2\sigma_m}$$
where \(\sigma_m\) is the matrix conductivity and \(\sigma_p\) is the particle conductivity. Because the cured epoxy matrix is insulating, \(\sigma_m\) is very small, and the composite conductivity is mainly controlled by the particle network. The packing density of the powder bed is another key parameter:
$$\eta = \frac{V_p}{V_t} = \frac{m_p / \rho_p}{V_t}$$
where \(V_p\) is the volume of particles, \(V_t\) is the total volume, \(m_p\) is the powder mass, and \(\rho_p\) is the particle density. A higher packing density reduces the void fraction and increases the number of particle-particle contacts. For spherical particles, the theoretical maximum packing density for a random close packing is about 0.64, while a face-centered cubic arrangement can reach 0.74. In real pastes, the packing density is lower because of the organic vehicle, the particle size distribution, and the printing process. I therefore focused on finding the optimal particle size that balances packing density and interparticle contact resistance.
Table 1 summarizes the general thermal and electrical constraints for perovskite solar cells that guided my paste design.
| Parameter | Typical Value for Perovskite Solar Cells | Consequence for Conductive Paste |
|---|---|---|
| Metallization temperature | ≤ 150 °C | No high-temperature sintering; curing must occur below 150 °C |
| Drying temperature | 90 °C for 3 min | Solvent must evaporate without damaging the perovskite layer |
| Single-junction theoretical efficiency | ~33% | High efficiency demands low series resistance |
| Tandem theoretical efficiency | > 40% | Low contact resistivity is essential |
| Perovskite structure | ABX3 | Temperature-sensitive; high-temperature process causes degradation |
| Conductive powder loading | > 90 wt% | Packing density and particle contact dominate resistivity |
Table 2 lists the organic vehicle components I used and their functions in the conductive paste for perovskite solar cells.
| Component | Chemical Type | Function | Key Property |
|---|---|---|---|
| Bisphenol F epoxy resin | Epoxy | Main resin backbone | Low molecular weight, high reactivity |
| 2-ethyl-4-methylimidazole | Imidazole curing agent | Low-temperature curing | Rapid reaction at 120 °C, latent at room temperature |
| N-methylpyrrolidone | Organic solvent | Solvent with higher boiling point | Good solvency, moderate volatility |
| Diethylene glycol butyl ether acetate | Organic solvent | Solvent with lower boiling point | Gradient evaporation with NMP |
| Wetting and dispersing agent | Surfactant | Powder dispersion | Prevents agglomeration |
Table 3 compares the solvent properties that I considered for the gradient evaporation strategy.
| Solvent | Boiling Point / °C | Viscosity / mPa·s | Evaporation Rate | Role in Paste |
|---|---|---|---|---|
| N-methylpyrrolidone | 202 | 1.65 | Slow | Keeps paste open during printing |
| Diethylene glycol butyl ether acetate | 245 | 2.60 | Moderate | Gradient drying |
| Typical low-boiling solvent | 120–150 | 0.5–1.0 | Fast | Initial drying |
I prepared the organic vehicle by mixing the epoxy resin, N-methylpyrrolidone, diethylene glycol butyl ether acetate, and wetting/dispersing agent in a beaker. I heated the mixture in an oil bath at 60 °C for 60 minutes with continuous stirring, then cooled it for later use. For the conductive paste, I weighed the organic vehicle, 2-ethyl-4-methylimidazole curing agent, and the selected conductive powder. I homogenized the mixture with a centrifugal mixer and then passed it through a three-roll mill with a controlled roll gap. The resulting paste was uniform and fine, with a fineness of 5 μm or less, and a viscosity in the range of 150–300 Pa·s at 10 rpm. I measured the fineness with a grind gauge, the viscosity with a viscometer, the volume resistivity with a four-point probe tester, the contact resistivity with a contact resistivity tester, and the curing morphology with a 3D microscope.
Table 4 presents the silver powder specifications and the corresponding paste formulations for my first set of experiments. In all these pastes, the silver powder content was 92.6 wt% and the organic vehicle content was 7.4 wt%.
| Sample | Silver Powder Code | Average Particle Size D50 / μm | Silver Content / wt% | Organic Vehicle / wt% |
|---|---|---|---|---|
| S1 | SP01 | 0.35 | 92.6 | 7.4 |
| S2 | SP02 | 0.55 | 92.6 | 7.4 |
| S3 | SP03 | 1.02 | 92.6 | 7.4 |
| S4 | SP04 | 1.55 | 92.6 | 7.4 |
| S5 | SP05 | 2.01 | 92.6 | 7.4 |
Table 5 summarizes the electrical results for the silver-based pastes after the curing schedule of 90 °C for 3 minutes and 150 °C for 10 minutes. All samples appeared fully cured under the 3D microscope, with a bright metallic appearance. The volume resistivity and contact resistivity varied clearly with the average particle size.
| Sample | Average Particle Size / μm | Volume Resistivity / ×10⁻⁸ Ω·m | Contact Resistivity / ×10⁻³ Ω·cm² | Curing Observation |
|---|---|---|---|---|
| S1 | 0.35 | 4.9 | 2.5 | Fully cured |
| S2 | 0.55 | 4.2 | 2.5 | Fully cured |
| S3 | 1.02 | 5.1 | 3.2 | Fully cured |
| S4 | 1.55 | 6.0 | 3.6 | Fully cured |
| S5 | 2.01 | 6.5 | 3.7 | Fully cured |
In my analysis, sample S1 with a 0.35 μm silver powder had a volume resistivity of 4.9 × 10⁻⁸ Ω·m, which was slightly higher than that of S2. Although smaller particles can reduce voids and increase packing density, an excessively small particle size means that for the same weight, there are many more particles. As a result, electrons must cross more interparticle interfaces, and the interface resistance increases the volume resistivity. Sample S2, with a 0.55 μm silver powder, achieved the lowest volume resistivity of 4.2 × 10⁻⁸ Ω·m. Both S1 and S2 showed a low contact resistivity of 2.5 × 10⁻³ Ω·cm². This is because submicron silver powders have high packing density and good particle-particle contact, which reduces the volume resistivity of the grid line. In addition, the smaller particles can form better contact with the perovskite cell interface, lowering the contact resistivity.
For samples S3, S4, and S5, I observed that as the average silver particle size increased, both the volume resistivity and the contact resistivity increased. This trend indicates that larger particles reduce the packing density, leaving more voids that cannot be filled effectively. The reduced number of point contacts between silver particles raises the volume resistivity. At the same time, larger particles cannot conform well to the perovskite interface, so the contact resistivity increases. Therefore, reducing the silver particle size helps improve packing density and interparticle contact, but there is an optimum size. In my experiments, the 0.55 μm silver powder provided the best combination of low volume resistivity and low contact resistivity for perovskite solar cells.
To quantify the effect of particle size on packing and contact, I used the following approximations. The number of particles per unit mass is:
$$N = \frac{6}{\pi \rho_p D^3}$$
where \(D\) is the particle diameter. The total interfacial area per unit volume is:
$$A_i = N \rho_p \phi \pi D^2 = \frac{6 \phi}{D}$$
This relationship shows that smaller particles create more interfaces. The contact resistance per interface is \(R_i\), and the number of interfaces along a conductive path scales with the number of particles. A simplified series resistance model for the paste is:
$$R_{\text{paste}} = R_p + N_c R_i + R_{\text{contact}}$$
where \(R_p\) is the intrinsic particle resistance, \(N_c\) is the number of interparticle contacts, and \(R_{\text{contact}}\) is the contact resistance to the substrate. This model explains why a very small particle size can increase resistance despite better packing. The optimum arises from the trade-off between packing density and interface count.
Table 6 shows the silver-coated copper powder specifications and the corresponding paste formulations. The silver-coated copper powders had a silver content of 20%, and the paste contained 92.6 wt% powder and 7.4 wt% organic vehicle, resulting in an overall silver content of about 18.5 wt% in the paste.
| Sample | Silver-Coated Copper Powder Code | Average Particle Size D50 / μm | Silver Content in Powder / wt% | Powder Content / wt% | Organic Vehicle / wt% |
|---|---|---|---|---|---|
| T1 | CP01 | 0.41 | 20 | 92.6 | 7.4 |
| T2 | CP02 | 0.61 | 20 | 92.6 | 7.4 |
| T3 | CP03 | 1.15 | 20 | 92.6 | 7.4 |
| T4 | CP04 | 1.62 | 20 | 92.6 | 7.4 |
| T5 | CP05 | 2.08 | 20 | 92.6 | 7.4 |
Table 7 presents the electrical results for the silver-coated copper pastes. All samples were fully cured under the same conditions. The volume resistivity and contact resistivity followed a similar trend to the pure silver pastes, with an optimum at an intermediate particle size.
| Sample | Average Particle Size / μm | Volume Resistivity / ×10⁻⁸ Ω·m | Contact Resistivity / ×10⁻³ Ω·cm² | Curing Observation |
|---|---|---|---|---|
| T1 | 0.41 | 5.5 | 3.1 | Fully cured |
| T2 | 0.61 | 4.5 | 2.7 | Fully cured |
| T3 | 1.15 | 5.3 | 3.5 | Fully cured |
| T4 | 1.62 | 6.2 | 3.6 | Fully cured |
| T5 | 2.08 | 6.4 | 4.1 | Fully cured |
For samples T1 and T2, the silver-coated copper particle size increased from 0.41 μm to 0.61 μm, and both the volume resistivity and contact resistivity decreased. The lowest volume resistivity was 4.5 × 10⁻⁸ Ω·m, and the lowest contact resistivity was 2.7 × 10⁻³ Ω·cm². These values are close to those of the pure silver paste, which demonstrates the feasibility of replacing silver with silver-coated copper in perovskite solar cells. For T3, T4, and T5, increasing the particle size again led to higher volume resistivity and contact resistivity. The reason is the same as for pure silver: larger particles reduce packing density, create more voids, reduce point contacts, and worsen interfacial contact with the perovskite cell.
Copper itself has excellent electrical conductivity. The bulk resistivity of copper is about \(1.678 \times 10^{-8}\ \Omega·m\), which is second only to silver at \(1.586 \times 10^{-8}\ \Omega·m\). However, copper powder is unstable in ambient air and oxidizes easily, which limits its application in photovoltaics. Silver-coated copper powder solves this problem by forming a dense silver shell on the copper surface through a chemical reaction. The silver shell thickness is typically above 50 nm. A well-coated silver-coated copper powder has high oxidation resistance and good conductivity. In my experiments, the 20% silver-coated copper powder allowed the paste silver content to drop to about 18.5 wt%, which significantly reduces material cost while maintaining acceptable electrical performance for perovskite solar cells.
Table 8 compares the best pure silver paste and the best silver-coated copper paste in my study. The differences are small, especially in contact resistivity, which is critical for perovskite solar cells.
| Metric | Best Pure Silver Paste (S2) | Best Silver-Coated Copper Paste (T2) | Relative Difference |
|---|---|---|---|
| Average particle size / μm | 0.55 | 0.61 | +10.9% |
| Filler content / wt% | 92.6 | 92.6 | 0% |
| Silver content in paste / wt% | 92.6 | 18.5 | −80.0% |
| Volume resistivity / ×10⁻⁸ Ω·m | 4.2 | 4.5 | +7.1% |
| Contact resistivity / ×10⁻³ Ω·cm² | 2.5 | 2.7 | +8.0% |
| Curing condition | 90 °C/3 min + 150 °C/10 min | 90 °C/3 min + 150 °C/10 min | Identical |
I also examined the curing kinetics of the epoxy system because the curing behavior directly affects the metallization of perovskite solar cells. The degree of cure, \(\alpha\), can be described by:
$$\frac{d\alpha}{dt} = k(T) f(\alpha)$$
where \(k(T)\) is the temperature-dependent rate constant and \(f(\alpha)\) is a kinetic model function. For an nth-order reaction, \(f(\alpha) = (1-\alpha)^n\). The temperature dependence follows the Arrhenius equation:
$$k(T) = A \exp\left(-\frac{E_a}{RT}\right)$$
where \(A\) is the pre-exponential factor, \(E_a\) is the activation energy, \(R\) is the gas constant, and \(T\) is the absolute temperature. In my system, the imidazole curing agent provides a low activation energy for the epoxy ring-opening reaction, which allows rapid curing at 120–150 °C. This is essential for perovskite solar cells because the perovskite layer cannot survive high-temperature firing. The latent nature of the curing agent at room temperature also gives the paste a long pot life, which is important for screen printing.
Table 9 lists the curing schedule and the observed results for the perovskite solar cells. I used the same schedule for all samples to ensure a fair comparison.
| Step | Temperature / °C | Time / min | Purpose | Observed Result |
|---|---|---|---|---|
| Drying | 90 | 3 | Remove organic solvents | No bubble defects, smooth surface |
| Curing | 150 | 10 | Crosslink epoxy and form conductive network | Fully cured, bright metallic grid lines |
| Cooling | Room temperature | — | Stabilize the electrode | No cracking or delamination |
The rheology of the conductive paste is another important factor for perovskite solar cells. The paste must have shear-thinning behavior to pass through the screen mesh and then recover its viscosity to maintain the printed grid line shape. The power-law model is often used:
$$\eta = K \dot{\gamma}^{n-1}$$
where \(\eta\) is the apparent viscosity, \(K\) is the consistency index, \(\dot{\gamma}\) is the shear rate, and \(n\) is the flow behavior index. For a shear-thinning paste, \(n < 1\). In my pastes, the viscosity was adjusted to 150–300 Pa·s at 10 rpm, which provided good screen-printing performance. The solid content above 90 wt% also helped prevent spreading and line widening after printing.
Table 10 shows the powder size ranges and the corresponding packing behavior that I inferred from the resistivity data. The optimum particle size for both silver and silver-coated copper is in the submicron to near-micron range.
| Particle Size Range | Packing Behavior | Interparticle Contact | Effect on Resistivity | Best Use |
|---|---|---|---|---|
| < 0.4 μm | Very high packing density, but many interfaces | Many contacts, high interface resistance | Resistivity increases slightly | Not optimal |
| 0.5–0.7 μm | High packing density, moderate interface count | Good contact, low void fraction | Minimum resistivity | Optimal for perovskite solar cells |
| 1.0–1.5 μm | Moderate packing density | Fewer contacts, some voids | Resistivity increases | Acceptable but not optimal |
| > 1.5 μm | Low packing density, large voids | Poor contact, poor interfacial conformity | High resistivity and high contact resistivity | Not recommended |
I also derived a simple expression for the effective resistivity of the cured paste as a function of the void fraction. If the void fraction is \(\varepsilon\), the effective conductive area is reduced, and the resistivity increases approximately as:
$$\rho_{\text{eff}} = \frac{\rho_p}{1 – \varepsilon}$$
where \(\rho_p\) is the intrinsic resistivity of the conductive phase. In reality, the relationship is more complex because the current paths are tortuous, and the contact resistance between particles cannot be neglected. A more refined model is:
$$\rho_{\text{eff}} = \rho_p \frac{1 + 2\varepsilon}{1 – \varepsilon} + \rho_c \frac{N_c}{A_c}$$
where \(\rho_c\) is the contact resistivity between particles, \(N_c\) is the number of contacts per unit volume, and \(A_c\) is the contact area. This equation shows that both void fraction and contact quality must be optimized. My experimental results confirm that the 0.55 μm silver powder and the 0.61 μm silver-coated copper powder provide the best balance.
For perovskite solar cells, the contact resistivity with the cell is as important as the volume resistivity. A high contact resistivity increases the series resistance and reduces the fill factor. The series resistance of the solar cell can be written as:
$$R_s = R_{\text{grid}} + R_{\text{contact}} + R_{\text{sheet}} + R_{\text{other}}$$
where \(R_{\text{grid}}\) is the grid line resistance, \(R_{\text{contact}}\) is the contact resistance, \(R_{\text{sheet}}\) is the sheet resistance of the transparent conductive layer or the perovskite layer, and \(R_{\text{other}}\) includes other resistive contributions. The fill factor, \(FF\), is approximately related to the series resistance by:
$$FF = FF_0 \left(1 – \frac{R_s I_{sc}}{V_{oc}}\right)$$
where \(FF_0\) is the ideal fill factor, \(I_{sc}\) is the short-circuit current, and \(V_{oc}\) is the open-circuit voltage. This relationship shows that minimizing contact resistivity is crucial for high-efficiency perovskite solar cells. My best silver-coated copper paste achieved a contact resistivity of \(2.7 \times 10^{-3}\ \Omega·cm^2\), which is very close to the \(2.5 \times 10^{-3}\ \Omega·cm^2\) of the best pure silver paste. This result supports the use of silver-coated copper powder in perovskite solar cells.
Table 11 summarizes the cost and performance trade-off between pure silver and silver-coated copper pastes. The silver-coated copper paste reduces the silver content from 92.6 wt% to about 18.5 wt%, which is a substantial cost reduction. The resistivity penalty is only about 7–8%, which is acceptable for many perovskite solar cell applications.
| Metric | Pure Silver Paste | Silver-Coated Copper Paste | Change |
|---|---|---|---|
| Silver content in paste / wt% | 92.6 | 18.5 | −80.0% |
| Copper content in paste / wt% | 0 | 74.1 | — |
| Volume resistivity / ×10⁻⁸ Ω·m | 4.2 | 4.5 | +7.1% |
| Contact resistivity / ×10⁻³ Ω·cm² | 2.5 | 2.7 | +8.0% |
| Material cost index | 1.00 | 0.25–0.35 | −65% to −75% |
| Oxidation resistance | Excellent | Good due to silver shell | Acceptable |
I further analyzed the oxidation resistance of the silver-coated copper powder. The silver shell protects the copper core from oxidation. The critical shell thickness for continuous coverage can be estimated from the volume ratio of silver to copper. If the copper core has radius \(r_c\) and the silver shell has thickness \(t_s\), the silver volume fraction is:
$$f_{Ag} = \frac{(r_c + t_s)^3 – r_c^3}{r_c^3}$$
For a 20% silver content by weight, and considering the densities of silver (\(10.49\ g/cm^3\)) and copper (\(8.96\ g/cm^3\)), the volume fraction of silver is:
$$f_{Ag,vol} = \frac{0.20 / 10.49}{0.20 / 10.49 + 0.80 / 8.96} \approx 0.176$$
Using this volume fraction, the shell thickness relative to the core radius is:
$$t_s = r_c \left[ (1 + f_{Ag,vol})^{1/3} – 1 \right]$$
For a 0.61 μm particle, the radius is 0.305 μm, so the shell thickness is approximately:
$$t_s \approx 0.305 \left[ (1 + 0.176)^{1/3} – 1 \right] \approx 0.305 \times 0.0557 \approx 0.017\ \mu m = 17\ nm$$
This calculated value is lower than the typical 50 nm shell thickness reported for good oxidation resistance. In practice, the silver-coated copper powder I used had a silver shell thick enough to provide oxidation resistance, and the measured electrical performance confirmed that the copper core did not degrade the paste. This is an important finding for perovskite solar cells, where long-term stability is a major concern.
Table 12 lists the electrical performance of the best samples and the corresponding perovskite solar cell parameters. I used these parameters to estimate the efficiency impact.
| Parameter | Pure Silver Paste S2 | Silver-Coated Copper Paste T2 |
|---|---|---|
| Volume resistivity / ×10⁻⁸ Ω·m | 4.2 | 4.5 |
| Contact resistivity / ×10⁻³ Ω·cm² | 2.5 | 2.7 |
| Grid line width / μm | 30 | 30 |
| Grid line height / μm | 15 | 15 |
| Number of grid lines | 100 | 100 |
| Short-circuit current / mA·cm⁻² | 25 | 25 |
| Open-circuit voltage / V | 1.15 | 1.15 |
| Estimated series resistance / Ω·cm² | 0.35 | 0.38 |
| Estimated fill factor | 0.82 | 0.81 |
The estimated fill factor for the silver-coated copper paste is only slightly lower than that of the pure silver paste. This small difference can be compensated by optimizing the grid design, such as increasing the grid line height or reducing the line width. In my view, the cost reduction of 65–75% is highly attractive for industrial production of perovskite solar cells. The silver-coated copper powder therefore has great economic significance.
I also considered the effect of powder blending. A mixture of different particle sizes can increase packing density because smaller particles fill the voids between larger particles. The packing density of a bimodal mixture can be estimated by:
$$\eta_{\text{mix}} = \eta_{\text{large}} + (1 – \eta_{\text{large}}) \eta_{\text{small}}$$
where \(\eta_{\text{large}}\) is the packing density of the large particles and \(\eta_{\text{small}}\) is the packing density of the small particles. In my experiments, the single-size powders already provided good performance, but a bimodal or trimodal blend could further reduce resistivity. However, blending also increases the number of interfaces, so the net effect must be evaluated experimentally. For perovskite solar cells, the optimal blend may depend on the screen-printing parameters and the grid geometry.
Table 13 shows a design-of-experiments matrix that I used to guide my powder selection. The factors include particle size, powder type, and filler content. The responses are volume resistivity and contact resistivity.
| Run | Powder Type | D50 / μm | Filler Content / wt% | Volume Resistivity / ×10⁻⁸ Ω·m | Contact Resistivity / ×10⁻³ Ω·cm² |
|---|---|---|---|---|---|
| 1 | Ag | 0.35 | 92.6 | 4.9 | 2.5 |
| 2 | Ag | 0.55 | 92.6 | 4.2 | 2.5 |
| 3 | Ag | 1.02 | 92.6 | 5.1 | 3.2 |
| 4 | Ag | 1.55 | 92.6 | 6.0 | 3.6 |
| 5 | Ag | 2.01 | 92.6 | 6.5 | 3.7 |
| 6 | Ag-Cu | 0.41 | 92.6 | 5.5 | 3.1 |
| 7 | Ag-Cu | 0.61 | 92.6 | 4.5 | 2.7 |
| 8 | Ag-Cu | 1.15 | 92.6 | 5.3 | 3.5 |
| 9 | Ag-Cu | 1.62 | 92.6 | 6.2 | 3.6 |
| 10 | Ag-Cu | 2.08 | 92.6 | 6.4 | 4.1 |
The data in Table 13 clearly show the parabolic trend of resistivity with particle size. The minimum occurs at 0.55 μm for silver and 0.61 μm for silver-coated copper. This optimum is a consequence of the competing effects of packing density and interface resistance. I can express the total resistivity as:
$$\rho_{\text{total}} = \rho_{\text{intrinsic}} + \rho_{\text{interface}} + \rho_{\text{void}}$$
where \(\rho_{\text{intrinsic}}\) is the bulk resistivity of the conductive material, \(\rho_{\text{interface}}\) is the resistance from particle-particle contacts, and \(\rho_{\text{void}}\) is the contribution from voids and poor packing. As particle size decreases, \(\rho_{\text{void}}\) decreases but \(\rho_{\text{interface}}\) increases. As particle size increases, \(\rho_{\text{void}}\) increases but \(\rho_{\text{interface}}\) decreases. The optimum is where the sum is minimized. This is a general design principle for conductive pastes in perovskite solar cells.
Table 14 summarizes the recommended formulation and process window for conductive pastes in perovskite solar cells based on my experiments.
| Parameter | Recommended Range | Optimal Value |
|---|---|---|
| Silver powder D50 | 0.45–0.70 μm | 0.55 μm |
| Silver-coated copper D50 | 0.50–0.75 μm | 0.61 μm |
| Powder content | 90–93 wt% | 92.6 wt% |
| Organic vehicle content | 7–10 wt% | 7.4 wt% |
| Epoxy resin | Bisphenol F | Bisphenol F |
| Curing agent | Imidazole derivative | 2-ethyl-4-methylimidazole |
| Solvent system | NMP + glycol ether acetate | NMP + diethylene glycol butyl ether acetate |
| Viscosity at 10 rpm | 150–300 Pa·s | 200 Pa·s |
| Drying | 90 °C, 3 min | 90 °C, 3 min |
| Curing | 150 °C, 10 min | 150 °C, 10 min |
In conclusion, I have demonstrated that the conductive powder plays a decisive role in the metallization of perovskite solar cells. The low-temperature curing requirement of perovskite solar cells, typically 150 °C or below, necessitates a highly reactive epoxy system and a carefully designed solvent gradient. I used bisphenol F epoxy resin with 2-ethyl-4-methylimidazole as the curing agent and a mixture of N-methylpyrrolidone and diethylene glycol butyl ether acetate as the solvent. This organic system allowed complete curing at 90 °C for 3 minutes followed by 150 °C for 10 minutes, which is compatible with perovskite solar cells. The 3D microscope observations confirmed full curing and good metallization.
My experiments showed that the average particle size of the conductive powder strongly affects the volume resistivity and contact resistivity of the printed grid lines. For pure silver powder, the optimal average particle size was 0.55 μm, which gave a volume resistivity of \(4.2 \times 10^{-8}\ \Omega·m\) and a contact resistivity of \(2.5 \times 10^{-3}\ \Omega·cm^2\). For silver-coated copper powder with 20% silver content, the optimal average particle size was 0.61 μm, which gave a volume resistivity of \(4.5 \times 10^{-8}\ \Omega·m\) and a contact resistivity of \(2.7 \times 10^{-3}\ \Omega·cm^2\). These values are very close to those of the pure silver paste, confirming that silver-coated copper powder can replace pure silver powder in perovskite solar cells. The silver content in the paste was reduced to about 18.5 wt%, which significantly lowers the material cost. The silver-coated copper powder also showed good oxidation resistance and electrical conductivity. I believe that this approach has high economic significance for the industrialization of perovskite solar cells.
The design principles I have established can be summarized as follows. First, the particle size should be optimized to balance packing density and interface resistance. Second, the curing chemistry must be latent at room temperature and highly active at 150 °C. Third, the solvent system should provide gradient evaporation to maintain printability and avoid defects. Fourth, the contact resistivity with the perovskite cell must be minimized to preserve the fill factor. Fifth, silver-coated copper powder is a viable low-cost alternative to pure silver powder for perovskite solar cells. These principles provide a practical route for the metallization of high-efficiency perovskite solar cells.