In our ongoing research into the safety and durability of energy storage systems, we have focused extensively on power-type lithium-ion batteries. These batteries are integral to modern applications due to their rapid charging capabilities, high power output, and long cycle life. However, as the power density of these li ion battery units increases, there is a noticeable compromise in their safety profiles. Mechanical abuse, such as external stress, can lead to internal short circuits caused by fractures in electrodes and separators, potentially resulting in thermal runaway, fires, or explosions. Therefore, a comprehensive understanding of the mechanical characteristics of battery components under external stress is crucial for both theoretical advancements and practical engineering applications.

Electrodes serve as the core components of any li ion battery, and their mechanical properties are key determinants of overall battery robustness. Previous studies have explored the relationship between electrode material fracture and electrochemical performance, examined novel materials like titanium diselenide monolayers for electrode applications, and investigated the mechanical behavior of anodes and current collectors. Notably, research has shown that binder elasticity affects electrode flexibility, and copper foil types exhibit different fracture modes. Additionally, the influence of charge-discharge cycles and strain rates on electrode mechanics has been documented, with findings indicating that higher cycling rates degrade tensile properties while slightly improving compression resistance. Moreover, electrodes in high-energy-density li ion battery cells demonstrate anisotropic behavior and strain-rate hardening. Despite these insights, most studies have concentrated on energy-type li ion battery cells, leaving a gap in understanding the mechanical responses of electrodes in power-type li ion battery systems, particularly concerning the effects of different active materials and state of charge (SOC).
In this study, we aim to address this gap by systematically examining the mechanical behavior of electrodes extracted from power-type 18650 lithium-ion batteries. Our approach involves tensile testing under varying strain rates and SOC levels, complemented by scanning electron microscopy (SEM) for microstructural analysis. Based on our experimental data, we develop a constitutive model to describe the strain-rate-dependent mechanical response of these electrodes. The insights gained are intended to inform the structural design and safety protocols for power-type li ion battery units, ensuring their reliability in demanding applications.
Experimental Methodology and Material Characterization
Our investigation centers on commercially available power-type 18650 cylindrical lithium-ion batteries. The core structure of these li ion battery cells consists of a jelly roll formed by winding negative electrodes, positive electrodes, and separators. The negative electrode uses copper foil as the current collector, coated with a composite active material primarily comprising graphite and soft carbon, bound together with a binder. The positive electrode employs aluminum foil coated with lithium nickel cobalt manganese oxide (NCM) as the active material. Key parameters of the test li ion battery are summarized in Table 1.
| Parameter | Value | Parameter | Value |
|---|---|---|---|
| Diameter (mm) | 18 | Negative Electrode Thickness (µm) | 120 ± 2 |
| Length (mm) | 65 | Positive Electrode Areal Density (g·cm⁻²) | 31 |
| Rated Capacity (mAh) | 1500 | Negative Electrode Areal Density (g·cm⁻²) | 15 |
| Voltage Range (V) | 2.5–4.2 | Positive Electrode Compaction Density (g·cm⁻³) | 3 |
| Fast-Charge Current (A) | 12 | Negative Electrode Compaction Density (g·cm⁻³) | 1.35 |
| Max. Continuous Discharge Current (A) | 15 | Aluminum Foil Thickness (µm) | 20 |
| Fast-Charge Cycle Life (cycles) | ≥8000 | Copper Foil Thickness (µm) | 9 |
| Positive Electrode Thickness (µm) | 120 ± 2 |
To prepare specimens for tensile testing, we carefully disassembled the li ion battery cells and extracted electrode sheets. These sheets were then cut into dog-bone-shaped samples using a custom-designed die. The sample geometry featured a gauge length of 12 mm, a width of 4 mm, and fillet radii of 6 mm. We defined three principal directions relative to the electrode rolling: 0° (axial direction), 90° (rolling direction), and 45° (intermediate direction). Tensile tests were conducted on a servo-hydraulic testing machine equipped with a 1 kN load cell and pneumatic grips. To prevent premature damage from grip pressure, rubber tabs were attached to the specimen ends.
Our experimental matrix was designed to probe two primary factors: strain-rate sensitivity and SOC dependence. For strain-rate effects, we tested both positive and negative electrodes along the 0°, 45°, and 90° directions at four distinct strain rates: $4 \times 10^{-5}$, $4 \times 10^{-4}$, $4 \times 10^{-3}$, and $4 \times 10^{-2}$ s⁻¹. Each test condition was replicated five times to ensure statistical reliability. To investigate SOC effects, we first charged separate li ion battery cells to specific SOC levels (0%, 20%, 40%, and 60%) using a constant current of 1C. After charging, these cells were disassembled, and electrode samples were extracted for tensile testing at a fixed strain rate of $4 \times 10^{-4}$ s⁻¹. Furthermore, to isolate the influence of active material, we prepared and tested electrodes with pure graphite and pure soft carbon anodes under the same SOC variations. Post-test, fracture surfaces and cross-sections of selected specimens were examined using SEM to correlate mechanical behavior with microstructural features.
Results and Analysis: Unraveling Electrode Mechanical Behavior
Anisotropic Nature of Electrodes
Our tensile tests immediately revealed that both positive and negative electrodes exhibit pronounced anisotropic mechanical properties. This means their strength varies significantly with direction relative to the rolling orientation. At a strain rate of $4 \times 10^{-3}$ s⁻¹, the stress-strain curves for all three directions demonstrated distinct failure stresses. For the positive electrode, the failure stress increased from approximately 30.19 MPa in the 0° direction to 31.12 MPa at 45° and 31.88 MPa at 90°. The failure strain remained relatively constant around 0.016. The negative electrode showed a similar trend, with failure stresses of 26.20 MPa (0°), 26.96 MPa (45°), and 27.76 MPa (90°), but with a larger failure strain of about 0.058. These results confirm that mechanical performance enhances from the axial to the rolling direction. The higher failure stress of the positive electrode compared to the negative indicates better load-bearing capacity, attributed to the aluminum current collector. Conversely, the larger failure strain of the negative electrode suggests greater ductility, likely due to the more ductile copper foil. This anisotropy is a critical factor in modeling the li ion battery response under multi-axial loading.
Strain-Rate Dependency and Hardening Effects
The mechanical response of both electrodes was strongly influenced by the applied strain rate, displaying clear strain-rate hardening. Figure 1 (represented conceptually) illustrates the stress-strain curves for the positive electrode at different strain rates. As the strain rate increased, the failure stress systematically rose while the failure strain diminished. This behavior was consistent across all tested directions for both electrodes. The negative electrode exhibited analogous trends, as summarized in Table 2, which consolidates key mechanical parameters extracted from the stress-strain curves.
| Direction | Strain Rate (s⁻¹) | Positive Electrode | Negative Electrode | ||||
|---|---|---|---|---|---|---|---|
| Elastic Modulus (GPa) | Yield Stress (MPa) | Failure Stress (MPa) | Elastic Modulus (GPa) | Yield Stress (MPa) | Failure Stress (MPa) | ||
| 0° | $4 \times 10^{-5}$ | 8.12 | 22.5 | 30.2 | 3.14 | 18.1 | 26.2 |
| $4 \times 10^{-4}$ | 8.85 | 24.1 | 31.8 | 3.45 | 19.3 | 27.5 | |
| $4 \times 10^{-3}$ | 9.32 | 25.3 | 32.9 | 3.78 | 20.5 | 28.7 | |
| $4 \times 10^{-2}$ | 9.91 | 26.8 | 34.2 | 4.05 | 21.8 | 29.8 | |
| 45° | $4 \times 10^{-5}$ | 8.34 | 23.1 | 31.1 | 3.28 | 18.7 | 27.0 |
| $4 \times 10^{-4}$ | 8.97 | 24.8 | 32.5 | 3.58 | 19.9 | 28.1 | |
| $4 \times 10^{-3}$ | 9.51 | 26.0 | 33.7 | 3.92 | 21.2 | 29.4 | |
| $4 \times 10^{-2}$ | 10.12 | 27.5 | 35.1 | 4.21 | 22.4 | 30.5 | |
| 90° | $4 \times 10^{-5}$ | 8.55 | 23.8 | 31.9 | 3.36 | 19.2 | 27.8 |
| $4 \times 10^{-4}$ | 9.18 | 25.4 | 33.3 | 3.67 | 20.4 | 29.0 | |
| $4 \times 10^{-3}$ | 9.74 | 26.7 | 34.6 | 4.01 | 21.7 | 30.2 | |
| $4 \times 10^{-2}$ | 10.38 | 28.3 | 36.0 | 4.32 | 23.0 | 31.4 | |
The data clearly shows that elastic modulus, yield stress, and failure stress all increase with higher strain rates for both electrodes in every direction. For instance, the elastic modulus of the positive electrode at 0° rose from 8.12 GPa at $4 \times 10^{-5}$ s⁻¹ to 9.91 GPa at $4 \times 10^{-2}$ s⁻¹. Similarly, the negative electrode’s elastic modulus increased from 3.14 GPa to 4.05 GPa over the same strain rate range. This strain-rate hardening is characteristic of many materials and is particularly important for li ion battery safety under dynamic loading conditions, such as in vehicular impacts.
SEM analysis of fracture surfaces provided microstructural insights. At lower strain rates, the electrode fractures showed more ductile features, with some delamination between the active material layer and the current collector. As the strain rate increased, the fracture surfaces became more brittle-looking, with increased cracking and greater detachment of active material particles. This degradation at high rates underscores the vulnerability of the electrode structure under rapid deformation, a key consideration for abuse tolerance in power-type li ion battery designs.
Influence of State of Charge on Mechanical Properties
The SOC of a li ion battery cell significantly affected the mechanical behavior of its electrodes, but the effect differed between positive and negative electrodes. For the positive electrode (NCM-based), tensile tests at SOC levels of 0%, 20%, 40%, and 60% revealed virtually identical stress-strain curves across all directions. This indicates that the mechanical properties of the positive electrode are largely independent of lithium concentration within the tested SOC range. In contrast, the negative electrode exhibited a strong SOC dependence. At SOC = 0%, the negative electrode displayed typical elastoplastic behavior with substantial ductility. However, as SOC increased to 20%, 40%, and 60%, the mechanical response gradually shifted. The failure stress increased, the failure strain decreased markedly, and at SOC ≥ 40%, the fracture mode transitioned to brittle failure with almost no plastic deformation. Measurements confirmed that the negative electrode thickness swelled from about 130 µm at SOC = 0% to 165 µm at SOC = 60%, indicating volumetric expansion due to lithium intercalation.
To delve deeper, we investigated electrodes with pure active materials. Table 3 lists the parameters for pure graphite and pure soft carbon anodes.
| Parameter | Pure Graphite Anode | Pure Soft Carbon Anode |
|---|---|---|
| Thickness (µm) | 100 | 100 |
| Particle Size (µm) | 9.4 | 14.63 |
| Binder | Polyvinylidene Fluoride (HSV900) | |
Tensile tests on these pure anodes revealed distinct behaviors. The pure soft carbon anode showed minimal change in its stress-strain response across different SOC levels, maintaining its elastoplastic character. This insensitivity is attributed to the amorphous structure of soft carbon, which has larger interlayer spacing that accommodates lithium ions without significant dimensional change or internal stress buildup. Conversely, the pure graphite anode mirrored the behavior of the composite negative electrode: at SOC = 0%, it was ductile; at higher SOC levels, it became increasingly brittle with higher strength. Graphite undergoes substantial lattice expansion (up to ~10% in volume) upon lithiation, generating significant internal stresses that harden the material and promote brittle fracture. This differential response highlights the critical role of active material selection in managing mechanical integrity across the operational SOC range of a li ion battery.
Development of a Constitutive Model for Strain-Rate Effects
To quantitatively capture the observed mechanical behavior, especially the strain-rate dependency, we developed a constitutive model based on the Ramberg-Osgood formulation. This model is well-suited for describing the elastoplastic response of materials. The basic form of the equation is:
$$ \epsilon = \frac{\sigma}{E} + a \times \left( \frac{\sigma}{b} \right)^n $$
where $\epsilon$ is the total strain, $\sigma$ is the stress, $E$ is the elastic modulus, and $a$, $b$, and $n$ are material constants determined from experimental data. To incorporate strain-rate effects, we modify the model by making $E$ and $b$ functions of the strain rate $\dot{\epsilon}$:
$$ \epsilon = \frac{\sigma}{E(\dot{\epsilon})} + a \times \left( \frac{\sigma}{b(\dot{\epsilon})} \right)^n $$
We focused on modeling the negative electrode behavior as an example (the positive electrode follows a similar procedure). Using the stress-strain data from the 0° direction at the reference strain rate of $4 \times 10^{-5}$ s⁻¹, we performed a nonlinear curve fit to determine the constants. The fitting yielded:
$$ a = 0.0109, \quad n = 22, \quad b_0 = 22.49 \, \text{MPa} $$
with a coefficient of determination $r^2 = 0.9971$, indicating an excellent fit. The comparison between experimental data and the fitted curve at this strain rate is shown conceptually in Figure 2. Next, keeping $a$ and $n$ fixed, we fitted the data at other strain rates to obtain the rate-dependent parameter $b(\dot{\epsilon})$. The values are listed in Table 4, along with the corresponding $E(\dot{\epsilon})$ values normalized to the reference modulus $E_0 = 3.14 \, \text{GPa}$.
| Strain Rate, $\dot{\epsilon}$ (s⁻¹) | $b(\dot{\epsilon})$ (MPa) | $E(\dot{\epsilon})$ / $E_0$ | Fitted $E(\dot{\epsilon})$ (GPa) |
|---|---|---|---|
| $4 \times 10^{-5}$ | 22.49 | 1.000 | 3.14 |
| $4 \times 10^{-4}$ | 23.43 | 1.098 | 3.45 |
| $4 \times 10^{-3}$ | 24.50 | 1.204 | 3.78 |
| $4 \times 10^{-2}$ | 25.02 | 1.290 | 4.05 |
The functional forms for $E(\dot{\epsilon})$ and $b(\dot{\epsilon})$ can be approximated by linear or power-law relationships. For instance, a linear fit for $b(\dot{\epsilon})$ in the log-strain rate domain might be used. The final model effectively predicts the stress-strain response across the tested strain rates, as verified by the close match between model predictions and experimental data for all rates. This constitutive model is a valuable tool for finite element simulations of li ion battery cells under mechanical abuse, enabling accurate prediction of internal stress states and potential failure initiation.
Comprehensive Discussion and Implications for Battery Design
The findings from this study have several important implications for the design and safety assessment of power-type lithium-ion batteries. First, the pronounced anisotropy underscores the need for direction-aware modeling when simulating battery deformation. Simplified isotropic models could lead to inaccurate predictions of failure locations and modes. Second, the strong strain-rate hardening effect indicates that electrodes become stiffer and stronger under dynamic loading. While this might offer some resistance to rapid deformation, the associated embrittlement at high rates, as seen in SEM, suggests a trade-off; the electrode may sustain higher stress but fail with less energy absorption through plastic deformation. This is critical for crashworthiness evaluations of electric vehicles where li ion battery packs may experience high-rate impacts.
The SOC-dependent behavior of the negative electrode, particularly its transition to brittle failure at high SOC, is a major safety concern. A fully charged li ion battery (high SOC) with a graphite-containing anode may be more susceptible to catastrophic internal short circuits under mechanical abuse due to this brittleness. In contrast, the SOC-insensitivity of the positive electrode and soft carbon anode suggests that material selection can mitigate this risk. Incorporating soft carbon or other materials with low expansion coefficients could enhance the mechanical robustness of the anode across the entire SOC window, thereby improving the overall safety of the li ion battery.
Our constitutive model provides a foundational framework for integrating electrode-level mechanical properties into larger-scale li ion battery module and pack simulations. The model parameters can be calibrated for different electrode compositions and manufacturing processes (e.g., calendering pressure affecting porosity). Furthermore, the model can be extended to incorporate SOC effects by making parameters functions of lithium concentration, although our data suggests this is primarily needed for graphite-based anodes.
Future work should explore the coupled electro-chemo-mechanical behavior more deeply. For instance, how does the mechanical damage (cracking, delamination) quantified in this study affect the ionic and electrical conductivity within the electrode, and consequently, the overall performance and aging of the li ion battery? Additionally, testing under more complex multi-axial stress states and at higher strain rates representative of extreme abuse scenarios would be valuable. Investigating the role of binder properties, as hinted by prior research, could also lead to optimized electrode formulations that balance mechanical integrity with electrochemical performance.
Conclusions
In this comprehensive investigation, we have systematically characterized the mechanical properties of electrodes extracted from commercial power-type 18650 lithium-ion batteries. Our key conclusions are as follows:
- Both positive and negative electrodes exhibit significant anisotropic mechanical behavior, with strength increasing from the axial (0°) to the rolling (90°) direction.
- The electrodes demonstrate strong strain-rate-dependent hardening. Elastic modulus, yield stress, and failure stress all increase with increasing strain rate, while failure strain decreases. Microstructural analysis via SEM confirms greater damage and brittle fracture features at higher strain rates.
- The state of charge has a negligible effect on the mechanical properties of the NCM-based positive electrode. However, for the composite negative electrode (graphite/soft carbon), increasing SOC leads to higher strength, reduced ductility, and a transition from ductile to brittle fracture at SOC levels above 40%. This is primarily driven by the volumetric expansion of graphite upon lithiation.
- Pure soft carbon anodes show minimal SOC-dependence in their mechanical response, whereas pure graphite anodes exhibit pronounced SOC-sensitive embrittlement, confirming the pivotal role of active material choice.
- We successfully developed a strain-rate-dependent constitutive model based on the Ramberg-Osgood formulation. The model, with parameters fitted from experimental data, accurately describes the elastoplastic response of the electrodes across a range of strain rates, providing a valuable tool for predictive simulation of li ion battery mechanical integrity.
These insights contribute substantially to the foundational knowledge required for designing safer and more robust power-type lithium-ion batteries. By accounting for anisotropy, strain-rate effects, and SOC-induced mechanical changes—especially in graphite anodes—engineers can develop better structural protections, select more suitable materials, and create more accurate simulation models to prevent failure in applications ranging from portable electronics to electric vehicles and grid storage. Ultimately, understanding and optimizing the mechanical behavior of electrodes is a crucial step toward advancing the reliability and safety of the ubiquitous li ion battery technology.