Unraveling Degradation in Lithium-ion Batteries: A Deep Dive Using the Distribution of Relaxation Times Method

The aging of lithium-ion batteries is governed by a complex interplay of physical and chemical degradation mechanisms. These mechanisms act on various internal components, leading to a gradual and often unpredictable decline in performance. Primarily, capacity fade in lithium-ion batteries stems from the loss of active lithium inventory—frequently due to side reactions or the growth of the Solid Electrolyte Interphase (SEI) layer—and the loss of active material in the electrodes, caused by phenomena such as structural disordering, particle cracking, and loss of electrical contact. As these mechanisms do not leave distinct, easily identifiable signatures on the macro-scale performance, developing comprehensive and precise diagnostic tools is crucial for a fundamental understanding of the aging process.

Electrochemical Impedance Spectroscopy (EIS) is a powerful technique widely used to probe the internal electrochemical processes of lithium-ion batteries. Conventionally, EIS data is analyzed by fitting to an Equivalent Circuit Model (ECM) to extract parameters linked to specific processes. However, a significant challenge lies in the clear separation of overlapping electrochemical processes in the frequency domain. In recent years, the Distribution of Relaxation Times (DRT) method has emerged as a transformative analytical tool. By deconvoluting the impedance spectrum into the time domain, the DRT method effectively separates polarization effects that typically overlap in conventional Nyquist plots, representing them as distinct peaks with specific amplitudes and time constants (τ). This peak-based representation offers a more intuitive and direct visualization of the complex physical processes occurring within the cell.

While studies have begun to explore the application of DRT for degradation analysis, limitations remain, particularly in the consistent attribution of DRT peaks to specific mechanisms across different stages of a battery’s lifecycle. This article presents a detailed methodology, employing a three-electrode cell configuration, to accurately attribute DRT peaks and correlate their evolution with the underlying aging mechanisms of a lithium nickel cobalt manganese oxide (LiNi0.5Co0.2Mn0.3O2 or NCM) / Graphite lithium-ion battery over extended cycling. The insights gained from monitoring these characteristic peaks are invaluable for developing more reliable State-of-Health (SOH) estimation algorithms.

Theoretical Foundation of the DRT Method

The core premise of the DRT analysis is that the impedance response of an electrochemical system, such as a lithium-ion battery, can be represented by a series connection of an ohmic resistor and an infinite number of parallel resistor-capacitor (RC) elements. Each RC element corresponds to a distinct electrochemical process with a unique time constant τ = RC. The overall impedance can be expressed as:

$$Z(j\omega) = R_{\text{ohmic}} + \int_{0}^{\infty} \frac{g(\tau)}{1 + j\omega\tau} d\tau$$

Where $Z$ is the complex impedance, $R_{\text{ohmic}}$ is the pure ohmic resistance, $j$ is the imaginary unit, $\omega$ is the angular frequency, and $g(\tau)$ is the distribution function of relaxation times. The function $g(\tau)$ is non-negative and encapsulates the relaxation characteristics of the system. The integral is often normalized, leading to:

$$Z(j\omega) = R_{\text{ohmic}} + R_{\text{pol}}\int_{0}^{\infty} \frac{\gamma(\tau)}{1 + j\omega\tau} d\tau$$

Here, $R_{\text{pol}}$ is the total polarization resistance, and $\gamma(\tau)$ represents the relative differential contribution of a single RC element. The DRT function $\gamma(\tau)$ (or $g(\tau)$) is what we compute from the EIS data. When plotted against $\tau$ or $\log(\tau)$, it appears as a series of peaks. Each peak’s position on the time-constant axis indicates the speed of the associated process (fast processes on the left, slow ones on the right), while its area (amplitude) is proportional to the polarization resistance of that process. For a lithium-ion battery, typical processes and their associated time constant ranges are categorized as follows:

Process Category Typical Time Constant Range (s) Physical Origin
Inductive/Electromagnetic Effects $\tau < 10^{-4}$ Cabling, cell windings, magnetic effects.
Ion Migration through Films $10^{-4} \leq \tau \leq 10^{-2}$ Li+ transport through the SEI on the anode or the CEI on the cathode.
Charge Transfer (Electrode Kinetics) $10^{-2} < \tau \leq 10^{1}$ Butler-Volmer kinetics at the electrode-electrolyte interface (both anode and cathode).
Solid-State Diffusion $\tau > 10^{1}$ Solid-state diffusion of Li+ within the active material particles (Warburg diffusion).

Experimental Methodology for Degradation Tracking

To achieve unambiguous peak attribution, a laboratory-made pouch cell with a three-electrode configuration was utilized. The working electrode was a graphite anode, the counter electrode was an NCM-based cathode, and a lithium metal reference electrode was established using an in-situ plating technique on a copper wire. This setup allows for independent measurement of the impedance for the full cell, the cathode vs. Li/Li+, and the anode vs. Li/Li+.

The lithium-ion battery was subjected to continuous cycle aging at 25°C using a standard 1C charge/1C discharge protocol between 2.80 V and 4.25 V. The aging progression was monitored until the capacity retention reached approximately 85%. At periodic intervals (every 100 cycles), comprehensive diagnostic tests were performed:

  1. EIS Measurements: Conducted at various States of Charge (SOC) from 0% to 100% (in 10% increments) for the full cell, cathode, and anode. A frequency range of 10 mHz to 1 MHz was employed.
  2. Low-Rate Characterization: Incremental Capacity (IC) and Differential Voltage (DV) analysis were performed using a low 0.1C rate to identify changes in the electrode-specific thermodynamic signatures.

Prior to DRT calculation, all EIS spectra were validated using the Kramers-Kronig (K-K) relations to ensure data consistency, stability, and linearity—a critical step for obtaining reliable and physically meaningful DRT results.

DRT Peak Attribution and Evolution During Aging

The DRT spectra for the full cell, cathode, and anode at a representative SOC (e.g., 40%) across different cycle numbers were computed and compared. This comparative analysis is key to deconvoluting the contributions from each electrode to the full-cell response. A consistent set of five primary peaks (labeled F1-F5 for the full cell, C1-C5 for the cathode, A1-A5 for the anode) was identified. Their attribution is summarized in the table below:

Peak Label Time Constant (τ) Range Attributed Process (Full Cell) Primary Electrode Contributor
F1 / C1 / A1 ~5×10-5 s Inductive/Electromagnetic effects Both electrodes & cell geometry.
F2 ~1×10-3 s Ion transport through surface films (SEI/CEI) Predominantly Anode (A2). Cathode film (C2) contribution is minor.
F3 3×10-2 – 8×10-2 s Charge Transfer at one electrode Predominantly Cathode (C3). Anode contribution (A3) is negligible.
F4 ~10-1 – 101 s Charge Transfer (mixed processes) Both Cathode (C4) and Anode (A4).
F5 > 10 s Solid-State Diffusion Both Cathode (C5) and Anode (A5).

The evolution of these peaks tells the story of the lithium-ion battery’s degradation:

  • Peak F1/A1/C1: Remained virtually unchanged throughout cycling, confirming it is related to static cell properties and not a degradation factor.
  • Peak F2 (Anode SEI): Showed a fluctuating but overall increasing trend in amplitude. This is consistent with the dynamic nature of the SEI layer, which may undergo repeated growth, partial dissolution, and reformation during cycling, leading to a net increase in ionic resistance over time.
  • Peak F3 (Cathode Charge Transfer): Exhibited the most significant and consistent growth in amplitude with cycling. The associated cathode peak (C3) also grew substantially and its time constant shifted to higher values. This is a clear indicator of the increasing kinetic hindrance at the cathode-electrolyte interface, suggesting phenomena like surface layer (CEI) growth, particle surface degradation, or loss of electrical contact.
  • Peak F4 (Mixed Charge Transfer): The amplitude of this peak also increased, driven mainly by the growth of the cathode component (C4). The anode charge transfer resistance (A4) remained relatively stable until very late stages of life.
  • Peak F5 (Diffusion): The amplitude increased progressively, indicating a general slowdown in solid-state diffusion kinetics, likely due to structural changes in the electrode materials.

To quantify these observations, the film resistance ($R_f$) and charge transfer resistance ($R_{ct}$) were extracted by integrating the areas under the relevant DRT peaks. $R_f$ is derived from the area of peak F2, while $R_{ct}$ is obtained from the combined area of peaks F3 and F4. The results plotted against SOC and cycle number reveal critical insights:

$$R_f^{\text{full}} \approx R_f^{\text{anode}}, \quad \text{relatively stable with cycling}$$
$$R_{ct}^{\text{full}} \approx R_{ct}^{\text{cathode}}, \quad \text{increases strongly with cycling, especially at low and high SOC}$$

This quantitative analysis solidifies the conclusion that the dominant factor in the impedance rise of this NCM/graphite lithium-ion battery is the deterioration of the cathode’s charge transfer kinetics, not the anode’s SEI growth. The anode’s health remains relatively stable until a potential “knee point” in degradation is approached at very high cycle counts.

Validation via Incremental Capacity and Differential Voltage Analysis

The degradation mechanisms inferred from the DRT analysis were cross-validated using thermodynamic techniques. Incremental Capacity (IC) and Differential Voltage (DV) analysis provide signatures related to phase transitions and stoichiometric changes in the electrode materials.

The IC curves of the full cell showed several characteristic peaks. Of particular interest are peaks associated with the cathode’s phase transitions (e.g., Ni2+/Ni3+/Ni4+ redox). The intensity of these cathode-related peaks diminished significantly over 900 cycles (e.g., a 44% decrease in one major peak), while peaks primarily influenced by the graphite anode showed much less change (e.g., only a 14% decrease late in life). This is direct evidence of active material loss and increasing disorder within the NCM cathode structure.

Similarly, Differential Voltage (DV) analysis of the three-electrode data allowed for the deconvolution of full-cell voltage plateaus into individual electrode contributions. The analysis confirmed that the shifts in the full-cell charge curves were predominantly due to the positive electrode’s potential curve shifting and distorting, indicative of lithium inventory loss and cathode active material degradation. The negative electrode’s DV features remained more stable.

The consistency between the kinetic picture from DRT (increasing cathode $R_{ct}$) and the thermodynamic picture from IC/DV (cathode active material loss) provides a robust and multi-faceted understanding of the primary aging mode in this lithium-ion battery.

Implications for Battery State of Health Estimation

The DRT method transforms complex EIS data into a set of trackable features (peak positions, amplitudes, areas) that are directly linked to underlying physical processes. This study demonstrates that for this chemistry, monitoring the amplitude of the charge-transfer related peaks—especially those originating from the cathode—provides a sensitive indicator of the lithium-ion battery’s State of Health (SOH).

This approach offers advantages over simple full-cell resistance measurements or ECM fitting:

  1. Process Isolation: It separates the contribution of the SEI from charge transfer and diffusion.
  2. Electrode-Level Diagnosis: When combined with a reference electrode or post-mortem analysis, it can pinpoint which electrode is degrading.
  3. Mechanistic Insight: The shape and shift of peaks can hint at specific failure modes (e.g., surface film growth vs. bulk structural disordering).

For practical SOH estimation, algorithms could be developed to extract key DRT features from periodic EIS measurements. A model could then correlate the evolution of, for example, the cathode charge transfer peak area with the remaining usable capacity of the lithium-ion battery. This represents a move towards more predictive and physics-based battery management.

Conclusions and Future Perspectives

This work has detailed an integrated methodology for analyzing the cycle aging of lithium-ion batteries, centering on the powerful DRT technique. By applying DRT to EIS data from a three-electrode pouch cell, we successfully deconvoluted the impedance spectrum, attributed specific peaks to anode SEI, cathode charge transfer, and mixed processes, and tracked their evolution over 900 cycles. The primary degradation mechanism was identified as cathode-driven, characterized by a significant increase in charge transfer resistance and correlated with active material loss observed in IC/DV analysis.

The DRT method proves to be an indispensable tool for moving beyond phenomenological aging models towards mechanism-oriented diagnosis. The ability to monitor distinct electrochemical processes through their characteristic time constants opens new avenues for:

  • Developing advanced BMS algorithms for precise SOH and Remaining Useful Life (RUL) prediction.
  • Guiding the design of more robust electrode materials and electrolytes by identifying the rate-limiting degradation processes.
  • Providing a standardized framework for comparing the aging behavior of different lithium-ion battery chemistries, such as Lithium Iron Phosphate (LFP) or Nickel-Cobalt-Aluminum (NCA).

Future research should focus on streamlining the DRT computation for potential embedded use, investigating its application under a wider range of aging conditions (e.g., calendar aging, low temperatures, fast charging), and establishing quantitative links between specific DRT feature changes and absolute capacity loss metrics. The pursuit of such deep diagnostic techniques is fundamental to enhancing the reliability, safety, and longevity of energy storage systems based on lithium-ion battery technology.

Scroll to Top